Category Polymer , Thermoplastic , Polystyrene (PS) , Polystyrene, Glass Filled
Manufacturer RTP Company
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF RTP Company RTP 401 FR Polystyrene (PS), Glass Fiber - Flame Retardant - UL94.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Physical Properties Metric English Comments
Specific Gravity 1.23 g/cc
1.23 g/cc
ASTM D 792
Filler Content 10 %
10 %
Primary Additive
Water Absorption 0.10 %
0.10 %
24 hrs @ 23°C; ASTM D 570
Linear Mold Shrinkage 0.0020 - 0.0030 cm/cm

@Thickness 3.17 mm
0.0020 - 0.0030 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 37.9 MPa
5500 psi
ASTM D 638
Elongation at Break 1.5 - 2.5 %
1.5 - 2.5 %
ASTM D 638
Tensile Modulus 4.14 GPa
600 ksi
ASTM D 638
Flexural Strength 62.1 MPa
9000 psi
ASTM D 790
Flexural Modulus 3.79 GPa
550 ksi
ASTM D 790
Izod Impact, Notched 0.534 J/cm

@Thickness 3.17 mm
1.00 ft-lb/in

@Thickness 0.125 in
D 256
Izod Impact, Unnotched 1.60 J/cm

@Thickness 3.17 mm
3.00 ft-lb/in

@Thickness 0.125 in
ASTM D4812
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 98.9 °C
210 °F
ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 82.2 °C
180 °F
ASTM D 648
Flammability, UL94 V-0

@Thickness 1.59 mm
V-0

@Thickness 0.0625 in
Electrical Properties Metric English Comments
Volume Resistivity >= 1.00e+16 ohm-cm
>= 1.00e+16 ohm-cm
ASTM D 257
Dielectric Strength 16.7 kV/mm
425 kV/in
Short Term; in oil; ASTM D 149
Processing Properties Metric English Comments
Melt Temperature 210 - 249 °C
410 - 480 °F
Mold Temperature 37.8 - 65.6 °C
100 - 150 °F
Drying Temperature 82.2 °C
180 °F
Dry Time 2 hour
2 hour
Injection Pressure 68.9 - 103 MPa
10000 - 15000 psi