Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Quadrant EPP Ketron® TX PEEK + solid lubricant, extruded (ISO Data)

Category Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) , Polyetheretherketone, PEEK, Unreinforced
Manufacturer Quadrant Engineering Plastics Products
Trade Name Ketron®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Quadrant EPP Ketron® TX PEEK + solid lubricant, extruded (ISO Data).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This member of the Ketron PEEK family has been developed especially for the food industry. Like Ketron PEEK-1000, this new internally lubricated material has a food contact compliant composition, but offers far superior wear and frictional performance making it especially suitable for a wide variety of bearing and wear applications in the 100 to 200 °C service temperature range. Very high maximum allowable service temperature in air (250 °C continuously, up to 310 °C for short periods of time) High mechanical strength, stiffness and creep resistance, also at elevated temperatures Excellent chemical and hydrolysis resistance Excellent wear & frictional behaviour Very good dimensional stability Excellent resistance to high energy radiation (gamma- and X-rays) Inherent low flammability and very low levels of smoke evolution during combustion
Physical Properties Metric English Comments
Density 1.39 g/cc
0.0502 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 0.18 %
0.18 %
50% RH
Water Absorption at Saturation 0.40 %
0.40 %
Mechanical Properties Metric English Comments
Hardness, Rockwell M 97
97
ISO 2039-2
Hardness, Shore D 85
85
Ball Indentation Hardness 195 MPa
28300 psi
ISO 2039-1
Tensile Strength 90.0 MPa
13100 psi
at Yield; ISO 527-1/-2
Elongation at Break 6.0 %
6.0 %
ISO 527-1/-2
Elongation at Yield 5.0 %
5.0 %
ISO 527-1/-2
Tensile Modulus 3.75 GPa
544 ksi
ISO 527-1/-2
Flexural Strength 140 MPa
20300 psi
Compressive Strength 31.0 MPa

@Strain 1 %
4500 psi

@Strain 1 %
ISO 604
61.0 MPa

@Strain 2 %
8850 psi

@Strain 2 %
ISO 604
120 MPa

@Strain 5 %
17400 psi

@Strain 5 %
ISO 604
K Factor (ISO) 9.0 µm/km
9.0 µm/km
Charpy Impact Unnotched 3.00 J/cm²
14.3 ft-lb/in²
ISO 179-1/1eU
Charpy Impact, Notched 0.300 J/cm²
1.43 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.25 - 0.35
0.25 - 0.35
Limiting Pressure Velocity 0.420 MPa-m/sec
12000 psi-ft/min
at 1 m/s unlubricated
0.660 MPa-m/sec
18800 psi-ft/min
at 0.1 m/s unlubricated
Thermal Properties Metric English Comments
CTE, linear 55.0 µm/m-°C

@Temperature 23.0 - 100 °C
30.6 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.250 W/m-K
1.74 BTU-in/hr-ft²-°F
Melting Point 340 °C
644 °F
DSC, 10°C/min.; ISO 11357-1/-3
Maximum Service Temperature, Air 250 °C
482 °F
Continuous
Deflection Temperature at 1.8 MPa (264 psi) 155 °C
311 °F
ISO 75-1/-2
Flammability, UL94 V-0
V-0
Oxygen Index 40 %
40 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+14 ohm-cm
>= 1.0e+14 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Constant 3.2

@Frequency >=100000 Hz
3.2

@Frequency >=100000 Hz
IEC 60250
Dielectric Strength 22.0 kV/mm
559 kV/in
Dissipation Factor 0.0010

@Frequency 100000 Hz
0.0010

@Frequency 100000 Hz
IEC 60250
Comparative Tracking Index 150 V
150 V
IEC 60112
Compliance Properties Metric English Comments
3A-Dairy No
No
European Food 1935/2004 Yes
Yes
FDA Yes
Yes
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Limited
Limited
Acids, Weak Acceptable
Acceptable
Alcohols Acceptable
Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Acceptable
Alkalies, Weak Acceptable
Acceptable
Chlorinated Solvents Acceptable
Acceptable
Continuous Sunlight Limited
Limited
Hot Water / Steam Acceptable
Acceptable
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Acceptable
Acceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Acceptable
Acceptable