Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Quadrant EPP Ketron® 1000 PEEK unfilled, extruded (ISO Data)

Category Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) , Polyetheretherketone, PEEK, Unreinforced
Manufacturer Quadrant Engineering Plastics Products
Trade Name Ketron®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Quadrant EPP Ketron® 1000 PEEK unfilled, extruded (ISO Data).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Ketron PEEK-1000 stock shapes are produced from virgin polyetheretherketone resin and offer the highest toughness and impact strength of all Ketron PEEK grades. Both Ketron PEEK-1000 natural & black can be sterilised by all conventional sterilisation methods (steam, dry heat, ethylene oxide and gamma irradiation). Very high maximum allowable service temperature in air (250 °C continuously, up to 310 °C for short periods of time) High mechanical strength, stiffness and creep resistance, also at elevated temperatures Excellent chemical and hydrolysis resistance Excellent wear & frictional behaviour Very good dimensional stability Excellent resistance to high energy radiation (gamma- and X-rays) Inherent low flammability and very low levels of smoke evolution during combustion
Physical Properties Metric English Comments
Density 1.31 g/cc
0.0473 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 0.20 %
0.20 %
50% RH
Water Absorption at Saturation 0.45 %
0.45 %
Outgassing - Total Mass Loss 0.26 %
0.26 %
Mechanical Properties Metric English Comments
Hardness, Rockwell M 105
105
ISO 2039-2
Hardness, Shore D 85
85
Ball Indentation Hardness 210 MPa
30500 psi
ISO 2039-1
Tensile Strength 115 MPa
16700 psi
at Yield; ISO 527-1/-2
Elongation at Break 17 %
17 %
ISO 527-1/-2
Elongation at Yield 5.0 %
5.0 %
ISO 527-1/-2
Tensile Modulus 4.30 GPa
624 ksi
ISO 527-1/-2
Flexural Strength 170 MPa
24700 psi
Compressive Strength 38.0 MPa

@Strain 1 %
5510 psi

@Strain 1 %
ISO 604
75.0 MPa

@Strain 2 %
10900 psi

@Strain 2 %
ISO 604
140 MPa

@Strain 5 %
20300 psi

@Strain 5 %
ISO 604
K Factor (ISO) 28 µm/km
28 µm/km
Charpy Impact Unnotched NB
NB
ISO 179-1/1eU
Charpy Impact, Notched 0.350 J/cm²
1.67 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.30 - 0.50
0.30 - 0.50
Limiting Pressure Velocity 0.210 MPa-m/sec
6000 psi-ft/min
at 1 m/s unlubricated
0.330 MPa-m/sec
9420 psi-ft/min
at 0.1 m/s unlubricated
Thermal Properties Metric English Comments
CTE, linear 50.0 µm/m-°C

@Temperature 23.0 - 100 °C
27.8 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.250 W/m-K
1.74 BTU-in/hr-ft²-°F
Melting Point 340 °C
644 °F
DSC, 10°C/min.; ISO 11357-1/-3
Maximum Service Temperature, Air 250 °C
482 °F
Continuous
Deflection Temperature at 1.8 MPa (264 psi) 160 °C
320 °F
ISO 75-1/-2
Flammability, UL94 V-0
V-0
Oxygen Index 35 %
35 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+14 ohm-cm
>= 1.0e+14 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Constant 3.2

@Frequency >=100000 Hz
3.2

@Frequency >=100000 Hz
IEC 60250
Dielectric Strength 24.0 kV/mm
610 kV/in
Dissipation Factor 0.0010

@Frequency 100000 Hz
0.0010

@Frequency 100000 Hz
IEC 60250
Comparative Tracking Index 150 V
150 V
IEC 60112
Compliance Properties Metric English Comments
3A-Dairy Yes
Yes
Only natural
European Food 1935/2004 Yes
Yes
natural and black
FDA Yes
Yes
natural and black
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Limited
Limited
Acids, Weak Acceptable
Acceptable
Alcohols Acceptable
Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Acceptable
Alkalies, Weak Acceptable
Acceptable
Chlorinated Solvents Acceptable
Acceptable
Continuous Sunlight Limited
Limited
Hot Water / Steam Acceptable
Acceptable
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Acceptable
Acceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Acceptable
Acceptable
Copyright © lookpolymers.com All Rights Reserved