Material Notes:
This material offers an optimal combination of mechanical strength, stiffness, toughness, mechanical damping properties and wear resistance. These properties, together with good electrical insulating properties and a good chemical resistance make Ertalon 6 SA a “general purpose” grade for mechanical construction and maintenance. High mechanical strength, stiffness, hardness and toughness Good fatigue resistance High mechanical damping ability Good sliding properties Excellent wear resistance Good electrical insulating properties Good resistance to high energy radiation (gamma- and X-rays) Good machinability
Physical Properties Metric English Comments
Density 1.14 g/cc
0.0412 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 2.6 %
2.6 %
50% RH
Water Absorption at Saturation 9.0 %
9.0 %
Outgassing - Total Mass Loss 1.3 %
1.3 %
Mechanical Properties Metric English Comments
Hardness, Rockwell M 85
85
ISO 2039-2
Hardness, Shore D 79
79
Ball Indentation Hardness 150 MPa
21800 psi
ISO 2039-1
Tensile Strength 80.0 MPa
11600 psi
at Yield; ISO 527-1/-2
Elongation at Break >= 50 %
>= 50 %
ISO 527-1/-2
Elongation at Yield 4.0 %
4.0 %
ISO 527-1/-2
Tensile Modulus 3.30 GPa
479 ksi
ISO 527-1/-2
Flexural Strength 116 MPa
16800 psi
Flexural Modulus 3.08 GPa
447 ksi
Compressive Strength 31.0 MPa

@Strain 1 %
4500 psi

@Strain 1 %
ISO 604
59.0 MPa

@Strain 2 %
8560 psi

@Strain 2 %
ISO 604
87.0 MPa

@Strain 5 %
12600 psi

@Strain 5 %
ISO 604
K Factor (ISO) 19 µm/km
19 µm/km
Charpy Impact Unnotched NB
NB
ISO 179-1/1eU
Charpy Impact, Notched 0.550 J/cm²
2.62 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.40 - 0.60
0.40 - 0.60
Limiting Pressure Velocity 0.0700 MPa-m/sec
2000 psi-ft/min
at 1 m/s unlubricated
0.120 MPa-m/sec
3430 psi-ft/min
at 0.1 m/s unlubricated
Thermal Properties Metric English Comments
CTE, linear 105 µm/m-°C

@Temperature 23.0 - 100 °C
58.3 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.280 W/m-K
1.94 BTU-in/hr-ft²-°F
Melting Point 220 °C
428 °F
DSC, 10°C/min.; ISO 11357-1/-3
Maximum Service Temperature, Air 70.0 °C
158 °F
Continuous; 20,000 h
85.0 °C
185 °F
Continuous; 5,000 h
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C
158 °F
ISO 75-1/-2
Flammability, UL94 HB
HB
Oxygen Index 25 %
25 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+14 ohm-cm
>= 1.0e+14 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Constant 3.9

@Frequency >=100000 Hz
3.9

@Frequency >=100000 Hz
IEC 60250
Dielectric Strength 25.0 kV/mm
635 kV/in
Dissipation Factor 0.019

@Frequency 100000 Hz
0.019

@Frequency 100000 Hz
IEC 60250
Comparative Tracking Index 600 V
600 V
IEC 60112
Compliance Properties Metric English Comments
3A-Dairy No
No
European Food 1935/2004 Yes
Yes
FDA Yes
Yes
only natural
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Unacceptable
Unacceptable
Acids, Weak Limited
Limited
Alcohols Limited
Limited
Alkalies, Strong (pH 11-14) Unacceptable
Unacceptable
Alkalies, Weak Limited
Limited
Chlorinated Solvents Limited
Limited
Continuous Sunlight Limited
Limited
Hot Water / Steam Limited
Limited
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Acceptable
Acceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Acceptable
Acceptable
Users viewing this material also viewed the following: