Proto3000 Duraform® GF Selective Laser Sintering (SLS®) Prototyping Polymer

Category Polymer , Rapid Prototyping Polymer , Thermoplastic , Nylon
Manufacturer Proto3000
Trade Name Duraform®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Proto3000 Duraform® GF Selective Laser Sintering (SLS®) Prototyping Polymer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Description: Glass-filled polyamide (nylon) material for real-world physical testing and functional useFeatures:Excellent mechanical stiffnessElevated temperature resistanceDimensionally stableEasy-to-processNice surface finishBenefits:Excels in load bearing applications at higher temperaturesBuild prototypes and end-use parts without toolingCreate accurate and repeatable parts as demanded by manufacturersMachinable and paintable for demonstration partsImproved isotropic shrinkage due to glass fillerApplications: Housings and enclosuresConsumer sporting goodsAppropriate for low- to mid-volume rapid manufacturingParts requiring machining or joining with adhesivesComplex production and prototype plastic partsForm, fit, or functional prototypesParts requiring stiffnessThermally stressed partsInformation provided by Proto3000 for their protoyping engineering services.
Physical Properties Metric English Comments
Density 1.49 g/cc
0.0538 lb/in³
ASTM D792
Water Absorption 22 %

@Time 86400 sec
22 %

@Time 24.0 hour
ASTM D570
Mechanical Properties Metric English Comments
Hardness, Shore D 77
77
ASTM D2240
Tensile Strength, Ultimate 26.0 MPa
3770 psi
ASTM D638
Tensile Strength, Yield 27.0 MPa
3920 psi
ASTM D638
Elongation at Break 1.4 %
1.4 %
ASTM D638
Elongation at Yield 1.4 %
1.4 %
ASTM D638
Tensile Modulus 4.068 GPa
590.0 ksi
ASTM D638
Flexural Strength 37.0 MPa
5370 psi
ASTM D790
Flexural Modulus 3.106 GPa
450.5 ksi
ASTM D790
Izod Impact, Notched 0.410 J/cm
0.768 ft-lb/in
ASTM D256
Izod Impact, Unnotched 1.23 J/cm
2.30 ft-lb/in
ASTM D256
Gardner Impact 4.50 J
3.32 ft-lb
ASTM D5420
Thermal Properties Metric English Comments
CTE, linear 82.6 µm/m-°C

@Temperature 0.000 - 50.0 °C
45.9 µin/in-°F

@Temperature 32.0 - 122 °F
ASTM E831
179.2 µm/m-°C

@Temperature 85.0 - 145 °C
99.56 µin/in-°F

@Temperature 185 - 293 °F
ASTM E831
Specific Heat Capacity 1.09 J/g-°C
0.261 BTU/lb-°F
ASTM E1269
Thermal Conductivity 0.470 W/m-K
3.26 BTU-in/hr-ft²-°F
ASTM E1225
Deflection Temperature at 0.46 MPa (66 psi) 179 °C
354 °F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 134 °C
273 °F
ASTM D648
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Volume Resistivity 3.20e+11 ohm-cm
3.20e+11 ohm-cm
ASTM D257
Surface Resistance 3.20e+11 ohm
3.20e+11 ohm
ASTM D257
Dielectric Constant 6.27

@Frequency 1.00e+6 Hz
6.27

@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 8.70 kV/mm
221 kV/in
ASTM D149
Dissipation Factor 0.177

@Frequency 1000 Hz
0.177

@Frequency 1000 Hz
ASTM D150