Material Notes:
OnFlex™ HFFR 315-01 a is non-halogen flame retardant material designed for flexible power cord insulation, cable jackets, and ribbon cables. New Product. Commercial specifications have not been established. - Non-halogen flame retardantPurge thoroughly before and after use of this product with a low flow (0.5 - 2.5 MFR) polyethylene (PE) or polypropylene (PP).Information provided by PolyOne
Physical Properties Metric English Comments
Specific Gravity 1.01 g/cc
1.01 g/cc
ASTM D792
Viscosity 26900 cP

@Shear Rate 11200 1/s,
Temperature 200 °C
26900 cP

@Shear Rate 11200 1/s,
Temperature 392 °F
ASTM D3835
1.86e+6 cP

@Shear Rate 67.0 1/s,
Temperature 200 °C
1.86e+6 cP

@Shear Rate 67.0 1/s,
Temperature 392 °F
ASTM D3835
Maximum Moisture Content 0.020
0.020
Deformation 42 %

@Temperature 150 °C
42 %

@Temperature 302 °F
2000g; UL 1581
Mechanical Properties Metric English Comments
Hardness, Shore A 75
75
10 sec; ASTM D2240
Tensile Strength at Break 20.7 MPa
3000 psi
UL 1581
13.4 MPa

@Temperature 23.0 °C
1940 psi

@Temperature 73.4 °F
Die C2 hr; ASTM D412
Elongation at Break 250 %
250 %
UL 1581
220 %

@Temperature 23.0 °C
220 %

@Temperature 73.4 °F
Die C2 hr; ASTM D412
Tear Strength 41.3 kN/m
236 pli
ASTM D624
Thermal Properties Metric English Comments
Brittleness Temperature -40.0 °C
-40.0 °F
ASTM D746
Electrical Properties Metric English Comments
Volume Resistivity 2.90e+15 ohm-cm

@Temperature 23.0 °C
2.90e+15 ohm-cm

@Temperature 73.4 °F
50%RH, ASTM D257-07; ASTM D257
Dielectric Strength 51.0 kV/mm

@Thickness 0.533 mm,
Temperature 23.0 °C
1300 kV/in

@Thickness 0.0210 in,
Temperature 73.4 °F
50% RH, ASTM D149-97a(04); ASTM D149
Processing Properties Metric English Comments
Zone 1 180 - 190 °C
356 - 374 °F
Zone 2 200 - 210 °C
392 - 410 °F
Zone 3 210 - 220 °C
410 - 428 °F
Zone 4 210 - 220 °C
410 - 428 °F
Die Temperature 210 - 220 °C
410 - 428 °F
Drying Temperature 70.0 °C
158 °F
Dry Time 2.00 - 3.00 hour
2.00 - 3.00 hour
Descriptive Properties Value Comments
Aging Resistance 100%
UL 1581; 136°C; Thermal aging tensile retention168hrs
85%
UL 1581; 136°C; Thermal aging elongation retension168hrs
Appearance Black
Features Flame Retardant
Forms Pellets
Generic Material TPE
Generic Name Thermoplastic Elastomer (TPE)
Manufacturer / Supplier GLS Thermoplastic Elastomers
Processing Method Extrusion
Regional Availability Africa & Middle East
Asia Pacific
Europe
North America
South America
Uses Cable Jacketing
Flexible Cord Insulation
Flexible Cord Jacketing
Wire & Cable Applications
VW-1 pass
UL 1581