Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Thermoplastic Polyurethane (TPUR), Polyester Grade

Category Polymer , Thermoplastic , Polyurethane, TP , Thermoplastic Polyurethane (TPUR), Polyester Grade
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Thermoplastic Polyurethane (TPUR), Polyester Grade.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Thermoplastic Polyurethane (TPUR), Polyester Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.650 - 1.44 g/cc
0.0235 - 0.0520 lb/in³
Average value: 1.20 g/cc Grade Count:332
Water Absorption 0.960 - 1.22 %
0.960 - 1.22 %
Average value: 1.09 % Grade Count:3
Moisture Absorption at Equilibrium 0.150 - 0.200 %
0.150 - 0.200 %
Average value: 0.183 % Grade Count:3
Water Absorption at Saturation 0.960 - 1.22 %
0.960 - 1.22 %
Average value: 1.09 % Grade Count:3
Viscosity 200 - 3500 cP
200 - 3500 cP
Average value: 1830 cP Grade Count:12
223000 - 223000 cP

@Temperature 204 - 204 °C
223000 - 223000 cP

@Temperature 399 - 399 °F
Average value: 223000 cP Grade Count:1
Maximum Moisture Content 0.0200 - 0.100
0.0200 - 0.100
Average value: 0.0450 Grade Count:12
Linear Mold Shrinkage 0.000700 - 0.0300 cm/cm
0.000700 - 0.0300 in/in
Average value: 0.00908 cm/cm Grade Count:37
Melt Flow 6.00 - 112 g/10 min
6.00 - 112 g/10 min
Average value: 34.0 g/10 min Grade Count:55
Mechanical Properties Metric English Comments
Hardness, Shore A 30.0 - 101
30.0 - 101
Average value: 83.5 Grade Count:301
74.0 - 75.0

@Temperature 70.0 - 100 °C
74.0 - 75.0

@Temperature 158 - 212 °F
Average value: 74.5 Grade Count:1
Hardness, Shore D 15.0 - 78.0
15.0 - 78.0
Average value: 50.7 Grade Count:149
Tensile Strength, Ultimate 0.800 - 80.0 MPa
116 - 11600 psi
Average value: 29.0 MPa Grade Count:318
4.05 - 26.63 MPa

@Temperature 70.0 - 100 °C
587 - 3862 psi

@Temperature 158 - 212 °F
Average value: 53.1 MPa Grade Count:1
45.0 - 45.0 MPa

@Temperature 136 - 136 °C
6530 - 6530 psi

@Temperature 277 - 277 °F
Average value: 53.1 MPa Grade Count:1
45.0 - 45.0 MPa

@Time 605000 - 605000 sec
6530 - 6530 psi

@Time 168 - 168 hour
Average value: 53.1 MPa Grade Count:1
24.0 - 102 MPa

@Strain 2.00 - 30.0 %
3480 - 14800 psi

@Strain 2.00 - 30.0 %
Average value: 53.1 MPa Grade Count:3
24.0 - 102 MPa

@Temperature 0.000 - 60.0 °C
3480 - 14800 psi

@Temperature 32.0 - 140 °F
Average value: 53.1 MPa Grade Count:3
Tensile Strength, Yield 0.552 - 900 MPa
80.0 - 131000 psi
Average value: 16.1 MPa Grade Count:244
2.60 - 4.00 MPa

@Temperature 70.0 - 100 °C
377 - 580 psi

@Temperature 158 - 212 °F
Average value: 3.43 MPa Grade Count:1
Elongation at Break 10.0 - 1000 %
10.0 - 1000 %
Average value: 548 % Grade Count:322
690 - 1080 %

@Temperature 70.0 - 100 °C
690 - 1080 %

@Temperature 158 - 212 °F
Average value: 758 % Grade Count:1
630 - 630 %

@Temperature 136 - 136 °C
630 - 630 %

@Temperature 277 - 277 °F
Average value: 758 % Grade Count:1
630 - 630 %

@Time 605000 - 605000 sec
630 - 630 %

@Time 168 - 168 hour
Average value: 758 % Grade Count:1
Elongation at Yield 320 - 850 %
320 - 850 %
Average value: 537 % Grade Count:36
Modulus of Elasticity 0.00260 - 1.90 GPa
0.377 - 276 ksi
Average value: 0.818 GPa Grade Count:8
0.00310 - 0.0917 GPa

@Temperature -50.0 - -20.0 °C
0.450 - 13.3 ksi

@Temperature -58.0 - -4.00 °F
Average value: 0.0264 GPa Grade Count:1
Flexural Modulus 0.00383 - 0.830 GPa
0.555 - 120 ksi
Average value: 0.124 GPa Grade Count:19
Resilience 20.0 - 55.0
20.0 - 55.0
Average value: 35.8 Grade Count:28
Rebound 1.21 - 60.0 %
1.21 - 60.0 %
Average value: 38.6 % Grade Count:23
Izod Impact, Notched 0.640 - 0.850 J/cm

@Temperature -40.0 - -40.0 °C
1.20 - 1.59 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 0.745 J/cm Grade Count:2
Charpy Impact Unnotched 10.0 - 1000 J/cm²
47.6 - 4760 ft-lb/in²
Average value: 13.4 J/cm² Grade Count:9
7.00 - 16.0 J/cm²

@Temperature -30.0 - -30.0 °C
33.3 - 76.1 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 10.2 J/cm² Grade Count:9
Charpy Impact, Notched 3.00 - 1000 J/cm²
14.3 - 4760 ft-lb/in²
Average value: 6.73 J/cm² Grade Count:48
0.300 - 999.9 J/cm²

@Temperature -30.0 - -30.0 °C
1.43 - 4759 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 3.59 J/cm² Grade Count:48
Tensile Creep Modulus, 1 hour 28.0 - 455 MPa
4060 - 66000 psi
Average value: 220 MPa Grade Count:3
Tensile Creep Modulus, 1000 hours 22.0 - 158 MPa
3190 - 22900 psi
Average value: 95.0 MPa Grade Count:3
Tear Strength 5.43 - 255 kN/m
31.0 - 1450 pli
Average value: 102 kN/m Grade Count:305
Graves Tear Strength 29.8 - 154 kN/m
170 - 880 pli
Average value: 78.2 kN/m Grade Count:5
K Factor (Wear Factor) 30.0 - 80.0
30.0 - 80.0
Average value: 51.8 Grade Count:36
Taber Abrasion, mg/1000 Cycles 5.00 - 146
5.00 - 146
Average value: 31.5 Grade Count:67
Compression Set 10.0 - 58.0 %
10.0 - 58.0 %
Average value: 24.8 % Grade Count:168
23.0 - 65.0 %

@Temperature 70.0 - 70.0 °C
23.0 - 65.0 %

@Temperature 158 - 158 °F
Average value: 46.2 % Grade Count:89
19.0 - 102 %

@Temperature 70.0 - 100 °C
19.0 - 102 %

@Temperature 158 - 212 °F
Average value: 46.2 % Grade Count:87
19.0 - 102 %

@Time 79200 - 252000 sec
19.0 - 102 %

@Time 22.0 - 70.0 hour
Average value: 46.2 % Grade Count:87
Tensile Set 4.00 - 19.0 %
4.00 - 19.0 %
Average value: 12.1 % Grade Count:5
Thermal Properties Metric English Comments
CTE, linear 15.0 - 224 µm/m-°C
8.33 - 124 µin/in-°F
Average value: 106 µm/m-°C Grade Count:20
Melting Point 71.0 - 225 °C
160 - 437 °F
Average value: 155 °C Grade Count:57
Deflection Temperature at 0.46 MPa (66 psi) 51.0 - 170 °C
124 - 338 °F
Average value: 119 °C Grade Count:13
Deflection Temperature at 1.8 MPa (264 psi) 39.0 - 130 °C
102 - 266 °F
Average value: 92.7 °C Grade Count:13
Vicat Softening Point 38.0 - 163 °C
100 - 325 °F
Average value: 94.5 °C Grade Count:63
Glass Transition Temp, Tg -53.9 - -13.9 °C
-65.0 - 7.00 °F
Average value: -35.3 °C Grade Count:39
Flammability, UL94 HB - V-2
HB - V-2
Grade Count:6
Optical Properties Metric English Comments
Transmission, Visible 85.0 - 90.0 %
85.0 - 90.0 %
Average value: 89.6 % Grade Count:12
Electrical Properties Metric English Comments
Electrical Resistivity 4.90e+10 - 5.00e+14 ohm-cm
4.90e+10 - 5.00e+14 ohm-cm
Average value: 6.77e+13 ohm-cm Grade Count:8
Surface Resistance 1.00e+8 - 9.00e+14 ohm
1.00e+8 - 9.00e+14 ohm
Average value: 8.27e+13 ohm Grade Count:11
Dielectric Constant 3.90 - 6.70
3.90 - 6.70
Average value: 5.39 Grade Count:8
Dielectric Strength 14.1 - 23.7 kV/mm
358 - 602 kV/in
Average value: 18.6 kV/mm Grade Count:8
Dissipation Factor 0.0111 - 0.0840
0.0111 - 0.0840
Average value: 0.0413 Grade Count:8
Users viewing this material also viewed the following: