Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polytetrafluoroethylene (PTFE), Carbon Fiber Filled

Category Polymer , Thermoplastic , Fluoropolymer , PTFE , Polytetrafluoroethylene (PTFE), Carbon Fiber Filled
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polytetrafluoroethylene (PTFE), Carbon Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polytetrafluoroethylene (PTFE), Carbon Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 2.00 - 2.65 g/cc
0.0723 - 0.0957 lb/in³
Average value: 2.14 g/cc Grade Count:21
Particle Size 25.0 - 800 µm
25.0 - 800 µm
Average value: 505 µm Grade Count:4
Mechanical Properties Metric English Comments
Hardness, Shore D 58.0 - 70.0
58.0 - 70.0
Average value: 62.5 Grade Count:12
Ball Indentation Hardness 38.0 - 56.0 MPa
5510 - 8120 psi
Average value: 50.3 MPa Grade Count:4
Tensile Strength, Ultimate 3.00 - 27.6 MPa
435 - 4000 psi
Average value: 16.6 MPa Grade Count:19
Tensile Strength, Yield 13.8 - 16.7 MPa
2000 - 2420 psi
Average value: 14.9 MPa Grade Count:3
Elongation at Break 3.00 - 350 %
3.00 - 350 %
Average value: 169 % Grade Count:22
Compressive Yield Strength 6.86 - 16.0 MPa
996 - 2320 psi
Average value: 9.98 MPa Grade Count:7
Shear Strength 10.3421 - 15.8579 MPa

@Temperature 26.7 - 204 °C
1500.00 - 2300.00 psi

@Temperature 80.0 - 400 °F
Average value: 12.5 MPa Grade Count:1
Coefficient of Friction 0.0800 - 0.160
0.0800 - 0.160
Average value: 0.123 Grade Count:11
Coefficient of Friction, Static 0.0800 - 0.300
0.0800 - 0.300
Average value: 0.142 Grade Count:10
Thermal Properties Metric English Comments
CTE, linear 75.0 - 150 µm/m-°C
41.7 - 83.3 µin/in-°F
Average value: 108 µm/m-°C Grade Count:3
100 - 223.2 µm/m-°C

@Temperature 30.0 - 300 °C
55.6 - 124.0 µin/in-°F

@Temperature 86.0 - 572 °F
Average value: 156 µm/m-°C Grade Count:2
Thermal Conductivity 0.260 - 0.988 W/m-K
1.80 - 6.86 BTU-in/hr-ft²-°F
Average value: 0.527 W/m-K Grade Count:11
0.290 - 0.310 W/m-K

@Temperature 100 - 250 °C
2.01 - 2.15 BTU-in/hr-ft²-°F

@Temperature 212 - 482 °F
Average value: 0.300 W/m-K Grade Count:1
Melting Point 327 °C
621 °F
Average value: 327 °C Grade Count:7
Maximum Service Temperature, Air 260 - 270 °C
500 - 518 °F
Average value: 263 °C Grade Count:10
Minimum Service Temperature, Air -260 - -50.0 °C
-436 - -58.0 °F
Average value: -131 °C Grade Count:10
Flammability, UL94 V-0
V-0
Grade Count:7
Electrical Properties Metric English Comments
Electrical Resistivity 100 - 1.00e+7 ohm-cm
100 - 1.00e+7 ohm-cm
Average value: 1.82e+6 ohm-cm Grade Count:11
Surface Resistance 1000 - 1.00e+7 ohm
1000 - 1.00e+7 ohm
Average value: 1.20e+6 ohm Grade Count:10
Copyright © lookpolymers.com All Rights Reserved