Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyphenylene Sulfide (PPS), NCG Fiber

Category Polymer , Thermoplastic , Polyphenylene Sulfide (PPS) , Polyphenylene Sulfide (PPS) + NGG
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyphenylene Sulfide (PPS), NCG Fiber.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "PPS + NGG". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.41 - 1.75 g/cc
0.0509 - 0.0632 lb/in³
Average value: 1.54 g/cc Grade Count:3
Filler Content 10.0 - 50.0 %
10.0 - 50.0 %
Average value: 25.0 % Grade Count:3
Water Absorption 0.00200 - 0.0200 %
0.00200 - 0.0200 %
Average value: 0.0140 % Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.00600 cm/cm
0.00100 - 0.00600 in/in
Average value: 0.00313 cm/cm Grade Count:3
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 55.2 - 172 MPa
8000 - 25000 psi
Average value: 113 MPa Grade Count:3
Elongation at Break 0.500 - 1.50 %
0.500 - 1.50 %
Average value: 0.900 % Grade Count:3
Modulus of Elasticity 8.27 - 28.3 GPa
1200 - 4100 ksi
Average value: 16.8 GPa Grade Count:3
Flexural Yield Strength 82.7 - 276 MPa
12000 - 40000 psi
Average value: 184 MPa Grade Count:3
Flexural Modulus 6.89 - 26.9 GPa
1000 - 3900 ksi
Average value: 15.9 GPa Grade Count:3
Izod Impact, Notched 0.267 - 0.801 J/cm
0.500 - 1.50 ft-lb/in
Average value: 0.498 J/cm Grade Count:3
Izod Impact, Unnotched 0.908 - 2.67 J/cm
1.70 - 5.00 ft-lb/in
Average value: 1.99 J/cm Grade Count:3
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 260 °C
500 °F
Average value: 260 °C Grade Count:3
Deflection Temperature at 1.8 MPa (264 psi) 232 - 260 °C
450 - 500 °F
Average value: 251 °C Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 0.100 - 10.0 ohm-cm
0.100 - 10.0 ohm-cm
Average value: 6.70 ohm-cm Grade Count:3
Processing Properties Metric English Comments
Processing Temperature 288 - 321 °C
550 - 610 °F
Average value: 304 °C Grade Count:3
Mold Temperature 135 - 177 °C
275 - 350 °F
Average value: 156 °C Grade Count:3
Injection Pressure 68.9 - 103 MPa
10000 - 15000 psi
Average value: 86.2 MPa Grade Count:3
Copyright © lookpolymers.com All Rights Reserved