Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyetheretherketone, Unreinforced

Category Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) , Polyetheretherketone, PEEK, Unreinforced
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyetheretherketone, Unreinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyetheretherketone, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.26 - 1.65 g/cc
0.0454 - 0.0596 lb/in³
Average value: 1.33 g/cc Grade Count:74
Filler Content 0.000 %
0.000 %
Average value: 0.000 % Grade Count:4
Water Absorption 0.0500 - 0.500 %
0.0500 - 0.500 %
Average value: 0.213 % Grade Count:25
Moisture Absorption at Equilibrium 0.100 - 0.500 %
0.100 - 0.500 %
Average value: 0.253 % Grade Count:12
Water Absorption at Saturation 0.100 - 1.65 %
0.100 - 1.65 %
Average value: 0.530 % Grade Count:23
0.550 - 0.560 %

@Temperature 100 - 100 °C
0.550 - 0.560 %

@Temperature 212 - 212 °F
Average value: 0.551 % Grade Count:7
Particle Size 10.0 - 70.0 µm
10.0 - 70.0 µm
Average value: 35.0 µm Grade Count:3
Viscosity 90000 - 380000 cP
90000 - 380000 cP
Average value: 183000 cP Grade Count:4
90000 - 500000 cP

@Temperature 400 - 400 °C
90000 - 500000 cP

@Temperature 752 - 752 °F
Average value: 324000 cP Grade Count:13
Linear Mold Shrinkage 0.00700 - 0.0180 cm/cm
0.00700 - 0.0180 in/in
Average value: 0.0108 cm/cm Grade Count:24
Linear Mold Shrinkage, Transverse 0.00900 - 0.0155 cm/cm
0.00900 - 0.0155 in/in
Average value: 0.0127 cm/cm Grade Count:12
Melt Flow 3.96 - 91.0 g/10 min
3.96 - 91.0 g/10 min
Average value: 32.0 g/10 min Grade Count:6
Spiral Flow 11.0 - 850 cm
4.33 - 335 in
Average value: 150 cm Grade Count:8
Mechanical Properties Metric English Comments
Hardness, Rockwell M 85.0 - 109
85.0 - 109
Average value: 102 Grade Count:18
Hardness, Rockwell R 120 - 127
120 - 127
Average value: 124 Grade Count:7
Hardness, Shore D 62.0 - 89.0
62.0 - 89.0
Average value: 84.6 Grade Count:19
Ball Indentation Hardness 90.0 - 230 MPa
13100 - 33400 psi
Average value: 192 MPa Grade Count:8
Tensile Strength, Ultimate 54.5 - 150 MPa
7900 - 21800 psi
Average value: 97.2 MPa Grade Count:42
25.0 - 80.0 MPa

@Temperature 60.0 - 150 °C
3630 - 11600 psi

@Temperature 140 - 302 °F
Average value: 55.0 MPa Grade Count:2
Tensile Strength, Yield 75.0 - 115 MPa
10900 - 16700 psi
Average value: 97.9 MPa Grade Count:28
Elongation at Break 1.50 - 110 %
1.50 - 110 %
Average value: 26.6 % Grade Count:67
30.0 - 45.0 %

@Temperature 60.0 - 150 °C
30.0 - 45.0 %

@Temperature 140 - 302 °F
Average value: 35.0 % Grade Count:2
Elongation at Yield 2.00 - 6.00 %
2.00 - 6.00 %
Average value: 4.45 % Grade Count:9
5.00 - 8.00 %

@Temperature 60.0 - 150 °C
5.00 - 8.00 %

@Temperature 140 - 302 °F
Average value: 6.00 % Grade Count:2
Modulus of Elasticity 2.20 - 6.48 GPa
319 - 940 ksi
Average value: 4.10 GPa Grade Count:62
3.00 - 3.70 GPa

@Temperature 60.0 - 150 °C
435 - 537 ksi

@Temperature 140 - 302 °F
Average value: 3.44 GPa Grade Count:2
Flexural Yield Strength 24.1 - 207 MPa
3500 - 30000 psi
Average value: 150 MPa Grade Count:55
9.00 - 90.0 MPa

@Temperature 125 - 275 °C
1310 - 13100 psi

@Temperature 257 - 527 °F
Average value: 42.2 MPa Grade Count:8
Flexural Modulus 3.50 - 6.89 GPa
508 - 1000 ksi
Average value: 4.15 GPa Grade Count:54
0.20312 - 0.20312 GPa

@Temperature 204 - 204 °C
29.460 - 29.460 ksi

@Temperature 400 - 400 °F
Average value: 0.203 GPa Grade Count:1
Compressive Yield Strength 31.0 - 183 MPa
4500 - 26500 psi
Average value: 108 MPa Grade Count:24
65.0 - 80.0 MPa

@Temperature 120 - 120 °C
9430 - 11600 psi

@Temperature 248 - 248 °F
Average value: 73.6 MPa Grade Count:7
Compressive Modulus 0.138 - 4.14 GPa
20.0 - 600 ksi
Average value: 2.97 GPa Grade Count:9
Shear Strength 55.2 - 82.7 MPa
8000 - 12000 psi
Average value: 67.3 MPa Grade Count:4
14.3411 - 68.2581 MPa

@Temperature 65.6 - 288 °C
2080.00 - 9900.02 psi

@Temperature 150 - 550 °F
Average value: 43.8 MPa Grade Count:1
Izod Impact, Notched 0.214 - 1.07 J/cm
0.400 - 2.00 ft-lb/in
Average value: 0.492 J/cm Grade Count:21
Izod Impact, Unnotched 13.3 - 25.6 J/cm
25.0 - 48.0 ft-lb/in
Average value: 20.1 J/cm Grade Count:3
Izod Impact, Notched (ISO) 0.450 - 9.50 kJ/m²
0.214 - 4.52 ft-lb/in²
Average value: 5.65 kJ/m² Grade Count:23
Izod Impact, Unnotched (ISO) NB
NB
Grade Count:23
Charpy Impact Unnotched 1.40 J/cm² - NB
6.66 ft-lb/in² - NB
Average value: 12.5 J/cm² Grade Count:21
Charpy Impact, Notched 0.300 - 8.00 J/cm²
1.43 - 38.1 ft-lb/in²
Average value: 0.889 J/cm² Grade Count:21
Coefficient of Friction 0.150 - 0.500
0.150 - 0.500
Average value: 0.279 Grade Count:17
K (wear) Factor 15.0 - 755 x 10-8 mm³/N-M
7.45 - 375 x 10-10 in³-min/ft-lb-hr
Average value: 472 x 10<sup>-8</sup> mm³/N-M Grade Count:9
Limiting Pressure Velocity 0.210 - 1.26 MPa-m/sec
6000 - 36000 psi-ft/min
Average value: 0.509 MPa-m/sec Grade Count:11
Compression Set 70.0 - 70.0 %

@Temperature 120 - 120 °C
70.0 - 70.0 %

@Temperature 248 - 248 °F
Average value: 70.0 % Grade Count:1
Thermal Properties Metric English Comments
CTE, linear 4.70 - 150 µm/m-°C
2.61 - 83.3 µin/in-°F
Average value: 51.6 µm/m-°C Grade Count:29
10.8 - 147.6 µm/m-°C

@Temperature 143 - 150 °C
6.00 - 82.00 µin/in-°F

@Temperature 289 - 302 °F
Average value: 122 µm/m-°C Grade Count:12
Electrical Properties Metric English Comments
Electrical Resistivity 15000 - 4.90e+16 ohm-cm
15000 - 4.90e+16 ohm-cm
Average value: 7.81e+15 ohm-cm Grade Count:34
1.00e+9 - 1.00e+15 ohm-cm

@Temperature 125 - 275 °C
1.00e+9 - 1.00e+15 ohm-cm

@Temperature 257 - 527 °F
Average value: 5.00e+14 ohm-cm Grade Count:8
Surface Resistance 3000 - 1.80e+15 ohm
3000 - 1.80e+15 ohm
Average value: 1.25e+14 ohm Grade Count:19
Dielectric Constant 2.20 - 10.9
2.20 - 10.9
Average value: 3.46 Grade Count:30
4.50 - 4.50

@Temperature 200 - 200 °C
4.50 - 4.50

@Temperature 392 - 392 °F
Average value: 4.50 Grade Count:3
4.50 - 4.50

@Frequency 50.0 - 50000 Hz
4.50 - 4.50

@Frequency 50.0 - 50000 Hz
Average value: 4.50 Grade Count:3
Dielectric Strength 15.7 - 200 kV/mm
400 - 5080 kV/in
Average value: 35.4 kV/mm Grade Count:30
Dissipation Factor 0.00100 - 0.518
0.00100 - 0.518
Average value: 0.0293 Grade Count:26
Comparative Tracking Index 150 - 175 V
150 - 175 V
Average value: 152 V Grade Count:14