Overview of materials for Polycarbonate, Extruded

Category Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate, Extruded
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polycarbonate, Extruded.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate, Extruded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.19 - 1.26 g/cc
0.0430 - 0.0455 lb/in³
Average value: 1.20 g/cc Grade Count:55
1.02 - 1.02 g/cc

@Temperature 290 - 310 °C
0.0368 - 0.0368 lb/in³

@Temperature 554 - 590 °F
Average value: 1.02 g/cc Grade Count:10
Water Absorption 0.0200 - 0.350 %
0.0200 - 0.350 %
Average value: 0.200 % Grade Count:29
Moisture Absorption at Equilibrium 0.120 - 0.200 %
0.120 - 0.200 %
Average value: 0.129 % Grade Count:18
Water Absorption at Saturation 0.300 - 0.400 %
0.300 - 0.400 %
Average value: 0.354 % Grade Count:12
Water Vapor Transmission 15.0 g/m²/day
0.966 g/100 in²/day
Average value: 15.0 g/m²/day Grade Count:4
Oxygen Transmission 65.0 - 70.0 cc-mm/m²-24hr-atm
165 - 178 cc-mil/100 in²-24hr-atm
Average value: 68.0 cc-mm/m²-24hr-atm Grade Count:4
Nitrogen Transmission 12.0 - 13.0 cc-mm/m²-24hr-atm
30.5 - 33.0 cc-mil/100 in²-24hr-atm
Average value: 12.5 cc-mm/m²-24hr-atm Grade Count:4
Carbon Dioxide Transmission 380 - 429 cc-mm/m²-24hr-atm
965 - 1090 cc-mil/100 in²-24hr-atm
Average value: 405 cc-mm/m²-24hr-atm Grade Count:4
Viscosity 800000 - 800000 cP

@Temperature 320 - 320 °C
800000 - 800000 cP

@Temperature 608 - 608 °F
Average value: 800000 cP Grade Count:1
800000 - 800000 cP

@Shear Rate 25.0 - 25.0 1/s
800000 - 800000 cP

@Shear Rate 25.0 - 25.0 1/s
Average value: 800000 cP Grade Count:1
Linear Mold Shrinkage 0.00200 - 0.00900 cm/cm
0.00200 - 0.00900 in/in
Average value: 0.00655 cm/cm Grade Count:33
Linear Mold Shrinkage, Transverse 0.00700 - 0.00800 cm/cm
0.00700 - 0.00800 in/in
Average value: 0.00780 cm/cm Grade Count:15
Melt Flow 1.00 - 18.0 g/10 min
1.00 - 18.0 g/10 min
Average value: 6.76 g/10 min Grade Count:44
Mechanical Properties Metric English Comments
Hardness, Rockwell M 70.0 - 75.0
70.0 - 75.0
Average value: 73.3 Grade Count:9
Hardness, Rockwell R 114 - 126
114 - 126
Average value: 120 Grade Count:15
Hardness, Shore D 79.0 - 80.0
79.0 - 80.0
Average value: 79.7 Grade Count:3
Ball Indentation Hardness 110 - 120 MPa
16000 - 17400 psi
Average value: 115 MPa Grade Count:7
Tensile Strength, Ultimate 60.0 - 74.0 MPa
8700 - 10700 psi
Average value: 68.0 MPa Grade Count:24
Tensile Strength, Yield 58.6 - 70.0 MPa
8500 - 10200 psi
Average value: 63.7 MPa Grade Count:34
Elongation at Break 10.0 - 138 %
10.0 - 138 %
Average value: 82.7 % Grade Count:41
Elongation at Yield 6.00 - 50.0 %
6.00 - 50.0 %
Average value: 11.9 % Grade Count:25
Modulus of Elasticity 1.79 - 3.24 GPa
260 - 470 ksi
Average value: 2.37 GPa Grade Count:27
Flexural Yield Strength 72.0 - 103 MPa
10400 - 15000 psi
Average value: 89.2 MPa Grade Count:24
Flexural Modulus 1.96 - 3.10 GPa
284 - 450 ksi
Average value: 2.32 GPa Grade Count:33
Compressive Yield Strength 18.0 - 86.2 MPa
2610 - 12500 psi
Average value: 60.4 MPa Grade Count:6
Compressive Modulus 2.07 GPa
300 ksi
Average value: 2.07 GPa Grade Count:3
Shear Strength 63.4 MPa
9200 psi
Average value: 63.4 MPa Grade Count:3
Izod Impact, Notched 0.481 - 9.61 J/cm
0.900 - 18.0 ft-lb/in
Average value: 6.71 J/cm Grade Count:27
5.00 - 5.00 J/cm

@Temperature 0.000 - 0.000 °C
9.37 - 9.37 ft-lb/in

@Temperature 32.0 - 32.0 °F
Average value: 3.86 J/cm Grade Count:2
2.72289 - 2.72289 J/cm

@Temperature -40.0 - -40.0 °C
5.10109 - 5.10109 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 3.86 J/cm Grade Count:1
2.72289 - 2.72289 J/cm

@Thickness 3.17 - 3.17 mm
5.10109 - 5.10109 ft-lb/in

@Thickness 0.125 - 0.125 in
Average value: 3.86 J/cm Grade Count:1
Izod Impact, Notched (ISO) 80.0 - 90.0 kJ/m²
38.1 - 42.8 ft-lb/in²
Average value: 82.5 kJ/m² Grade Count:4
12.0 - 14.0 kJ/m²

@Temperature -30.0 - -30.0 °C
5.71 - 6.66 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 13.0 kJ/m² Grade Count:4
12.0 - 14.0 kJ/m²

@Thickness 3.20 - 3.20 mm
5.71 - 6.66 ft-lb/in²

@Thickness 0.126 - 0.126 in
Average value: 13.0 kJ/m² Grade Count:4
Charpy Impact Unnotched 1000 J/cm² - NB
4760 ft-lb/in² - NB
Grade Count:23
999.9 J/cm² - NB

@Temperature -60.0 - -30.0 °C
4759 ft-lb/in² - NB

@Temperature -76.0 - -22.0 °F
Grade Count:14
Charpy Impact, Notched 0.900 - 8.00 J/cm²
4.28 - 38.1 ft-lb/in²
Average value: 4.73 J/cm² Grade Count:7
1.40 - 1.60 J/cm²

@Temperature -30.0 - -30.0 °C
6.66 - 7.61 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 1.50 J/cm² Grade Count:4
1.40 - 1.60 J/cm²

@Thickness 3.00 - 3.00 mm
6.66 - 7.61 ft-lb/in²

@Thickness 0.118 - 0.118 in
Average value: 1.50 J/cm² Grade Count:4
Gardner Impact 36.2 J
26.7 ft-lb
Average value: 36.2 J Grade Count:3
Puncture Energy 50.0 - 65.0 J
36.9 - 47.9 ft-lb
Average value: 58.9 J Grade Count:14
55.0 - 75.0 J

@Temperature -30.0 - -30.0 °C
40.6 - 55.3 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 66.4 J Grade Count:14
Coefficient of Friction 0.500 - 0.600
0.500 - 0.600
Average value: 0.533 Grade Count:3
Tensile Creep Modulus, 1 hour 2200 MPa
319000 psi
Average value: 2200 MPa Grade Count:12
Tensile Creep Modulus, 1000 hours 1900 MPa
276000 psi
Average value: 1900 MPa Grade Count:12
Thermal Properties Metric English Comments
CTE, linear 50.0 - 70.2 µm/m-°C
27.8 - 39.0 µin/in-°F
Average value: 65.5 µm/m-°C Grade Count:29
CTE, linear, Transverse to Flow 65.0 - 70.0 µm/m-°C
36.1 - 38.9 µin/in-°F
Average value: 65.5 µm/m-°C Grade Count:16
Electrical Properties Metric English Comments
Electrical Resistivity 1000 - 1.00e+17 ohm-cm
1000 - 1.00e+17 ohm-cm
Average value: 1.27e+16 ohm-cm Grade Count:31
Surface Resistance 10000 - 1.00e+16 ohm
10000 - 1.00e+16 ohm
Average value: 3.92e+15 ohm Grade Count:26
Dielectric Constant 2.85 - 3.17
2.85 - 3.17
Average value: 3.02 Grade Count:26
Dielectric Strength 15.0 - 34.0 kV/mm
380 - 864 kV/in
Average value: 29.6 kV/mm Grade Count:27
Dissipation Factor 0.000500 - 0.0400
0.000500 - 0.0400
Average value: 0.00669 Grade Count:26
Arc Resistance 120 sec
120 sec
Average value: 120 sec Grade Count:6
Comparative Tracking Index 100 - 350 V
100 - 350 V
Average value: 224 V Grade Count:16