Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "PVC, 20% Glass Fiber Reinforced". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.50 - 1.55 g/cc
0.0542 - 0.0560 lb/in³
Average value: 1.52 g/cc Grade Count:4
Linear Mold Shrinkage 0.000 - 0.0150 cm/cm
0.000 - 0.0150 in/in
Average value: 0.00533 cm/cm Grade Count:3
Mechanical Properties Metric English Comments
Hardness, Shore D 83.0 - 85.0
83.0 - 85.0
Average value: 83.8 Grade Count:4
Modulus of Elasticity 6.55 - 7.03 GPa
950 - 1020 ksi
Average value: 6.76 GPa Grade Count:4
Flexural Yield Strength 96.1 - 138 MPa
13900 - 20000 psi
Average value: 110 MPa Grade Count:4
Flexural Modulus 6.20 - 6.43 GPa
899 - 933 ksi
Average value: 6.26 GPa Grade Count:4
Poissons Ratio 0.410 - 0.420
0.410 - 0.420
Average value: 0.417 Grade Count:3
Shear Modulus 2.31 - 2.43 GPa
335 - 352 ksi
Average value: 2.35 GPa Grade Count:3
Izod Impact, Notched 0.160 - 0.907 J/cm
0.300 - 1.70 ft-lb/in
Average value: 0.527 J/cm Grade Count:4
Izod Impact, Unnotched 3.20 - 5.30 J/cm
5.99 - 9.93 ft-lb/in
Average value: 4.26 J/cm Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 27.0 - 31.0 µm/m-°C
15.0 - 17.2 µin/in-°F
Average value: 28.5 µm/m-°C Grade Count:4
Deflection Temperature at 1.8 MPa (264 psi) 72.8 - 77.2 °C
163 - 171 °F
Average value: 75.3 °C Grade Count:4
Processing Properties Metric English Comments
Melt Temperature 188 - 210 °C
370 - 410 °F
Average value: 200 °C Grade Count:4
Users viewing this material also viewed the following: