Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Impact Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.03 - 1.46 g/cc
0.0372 - 0.0527 lb/in³
Average value: 1.11 g/cc Grade Count:301
0.950 - 0.950 g/cc

@Temperature 285 - 285 °C
0.0343 - 0.0343 lb/in³

@Temperature 545 - 545 °F
Average value: 0.950 g/cc Grade Count:1
Water Absorption 0.400 - 8.00 %
0.400 - 8.00 %
Average value: 1.81 % Grade Count:144
Moisture Absorption at Equilibrium 0.170 - 3.10 %
0.170 - 3.10 %
Average value: 2.10 % Grade Count:76
Water Absorption at Saturation 5.50 - 9.00 %
5.50 - 9.00 %
Average value: 6.77 % Grade Count:19
Linear Mold Shrinkage 0.00150 - 0.0350 cm/cm
0.00150 - 0.0350 in/in
Average value: 0.0158 cm/cm Grade Count:263
Linear Mold Shrinkage, Transverse 0.00800 - 0.0302 cm/cm
0.00800 - 0.0302 in/in
Average value: 0.0171 cm/cm Grade Count:78
Melt Flow 1.00 - 2.00 g/10 min
1.00 - 2.00 g/10 min
Average value: 1.81 g/10 min Grade Count:10
Spiral Flow 0.800 - 77.0 cm
0.315 - 30.3 in
Average value: 51.6 cm Grade Count:3
Mechanical Properties Metric English Comments
Hardness, Rockwell M 60.0 - 93.0
60.0 - 93.0
Average value: 76.4 Grade Count:14
Hardness, Rockwell R 69.0 - 120
69.0 - 120
Average value: 108 Grade Count:95
Hardness, Shore D 70.0 - 81.0
70.0 - 81.0
Average value: 73.7 Grade Count:6
Ball Indentation Hardness 80.0 - 160 MPa
11600 - 23200 psi
Average value: 114 MPa Grade Count:10
Tensile Strength, Ultimate 20.7 - 331 MPa
3000 - 48000 psi
Average value: 58.7 MPa Grade Count:190
Tensile Strength, Yield 35.0 - 155 MPa
5080 - 22500 psi
Average value: 58.5 MPa Grade Count:161
Elongation at Break 1.00 - 260 %
1.00 - 260 %
Average value: 55.5 % Grade Count:260
>= 100 %

@Temperature 60.0 - 150 °C
>= 100 %

@Temperature 140 - 302 °F
Average value: 100 % Grade Count:1
Elongation at Yield 2.00 - 210 %
2.00 - 210 %
Average value: 23.6 % Grade Count:67
Modulus of Elasticity 0.600 - 41.4 GPa
87.0 - 6000 ksi
Average value: 2.65 GPa Grade Count:125
0.170 - 2.716 GPa

@Temperature -40.0 - 150 °C
24.7 - 393.9 ksi

@Temperature -40.0 - 302 °F
Average value: 0.783 GPa Grade Count:2
Flexural Yield Strength 17.0 - 507 MPa
2470 - 73500 psi
Average value: 79.8 MPa Grade Count:236
15.0 - 15.0 MPa

@Temperature 90.0 - 90.0 °C
2180 - 2180 psi

@Temperature 194 - 194 °F
Average value: 15.0 MPa Grade Count:1
Flexural Modulus 0.0700 - 36.2 GPa
10.2 - 5250 ksi
Average value: 2.51 GPa Grade Count:279
0.300 - 0.300 GPa

@Temperature 90.0 - 90.0 °C
43.5 - 43.5 ksi

@Temperature 194 - 194 °F
Average value: 0.300 GPa Grade Count:1
Compressive Yield Strength 30.3 - 100 MPa
4400 - 14500 psi
Average value: 63.5 MPa Grade Count:6
Shear Modulus >= 0.0219 GPa

@Temperature -50.0 - 250 °C
>= 3.18 ksi

@Temperature -58.0 - 482 °F
Average value: 0.318 GPa Grade Count:1
Shear Strength 41.0 - 57.0 MPa
5950 - 8270 psi
Average value: 49.0 MPa Grade Count:4
Izod Impact, Notched 0.481 - 5340 J/cm
0.900 - 10000 ft-lb/in
Average value: 5.07 J/cm Grade Count:165
0.300 - 5.339 J/cm

@Temperature -40.0 - -40.0 °C
0.562 - 10.00 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 1.51 J/cm Grade Count:5
0.5339 - 2.6695 J/cm

@Temperature -40.0 - 72.8 °C
1.000 - 5.0011 ft-lb/in

@Temperature -40.0 - 163 °F
Average value: 1.51 J/cm Grade Count:18
0.5339 - 2.6695 J/cm

@Thickness 3.17 - 3.17 mm
1.000 - 5.0011 ft-lb/in

@Thickness 0.125 - 0.125 in
Average value: 1.51 J/cm Grade Count:18
Izod Impact, Unnotched 0.430 J/cm - NB
0.806 ft-lb/in - NB
Average value: 8.83 J/cm Grade Count:45
Izod Impact, Notched (ISO) 10.0 kJ/m² - NB
4.76 ft-lb/in² - NB
Average value: 47.3 kJ/m² Grade Count:80
8.00 - 90.0 kJ/m²

@Temperature -40.0 - -20.0 °C
3.81 - 42.8 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 24.1 kJ/m² Grade Count:52
Izod Impact, Unnotched (ISO) 96.0 kJ/m² - NB
45.7 ft-lb/in² - NB
Average value: 97.0 kJ/m² Grade Count:12
NB - NB

@Temperature -30.0 - -30.0 °C
NB - NB

@Temperature -22.0 - -22.0 °F
Grade Count:5
Charpy Impact Unnotched 9.00 J/cm² - NB
42.8 ft-lb/in² - NB
Average value: 13.2 J/cm² Grade Count:93
4.40 J/cm² - NB

@Temperature -40.0 - -20.0 °C
20.9 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 8.98 J/cm² Grade Count:68
Charpy Impact, Notched 0.450 J/cm² - NB
2.14 ft-lb/in² - NB
Average value: 4.74 J/cm² Grade Count:102
0.450 - 6.50 J/cm²

@Temperature -40.0 - -20.0 °C
2.14 - 30.9 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 2.06 J/cm² Grade Count:72
Gardner Impact 36.2 - 38.0 J
26.7 - 28.0 ft-lb
Average value: 36.5 J Grade Count:5
12.2024 - 12.2024 J

@Temperature -40.0 - -40.0 °C
9.00001 - 9.00001 ft-lb

@Temperature -40.0 - -40.0 °F
Average value: 12.2 J Grade Count:1
Dart Drop, Total Energy 50.0 - 50.0 J

@Temperature -20.0 - -20.0 °C
36.9 - 36.9 ft-lb

@Temperature -4.00 - -4.00 °F
Average value: 50.0 J Grade Count:1
Tensile Creep Modulus, 1000 hours 400 - 840 MPa
58000 - 122000 psi
Average value: 663 MPa Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 1.00 - 1.00e+16 ohm-cm
1.00 - 1.00e+16 ohm-cm
Average value: 1.16e+15 ohm-cm Grade Count:126
Surface Resistance 1.00 - 1.00e+16 ohm
1.00 - 1.00e+16 ohm
Average value: 8.14e+14 ohm Grade Count:69
Static Decay 1.00 - 2.00 sec
1.00 - 2.00 sec
Average value: 1.67 sec Grade Count:3
Dielectric Constant 2.70 - 10.0
2.70 - 10.0
Average value: 3.78 Grade Count:58
Dielectric Strength 9.84 - 120 kV/mm
250 - 3050 kV/in
Average value: 31.2 kV/mm Grade Count:101
Dissipation Factor 0.00670 - 0.200
0.00670 - 0.200
Average value: 0.0361 Grade Count:25
Dielectric Loss Index 0.0130 - 0.130
0.0130 - 0.130
Average value: 0.0469 Grade Count:9
Arc Resistance 60.0 - 179 sec
60.0 - 179 sec
Average value: 108 sec Grade Count:20
Comparative Tracking Index 525 - 600 V
525 - 600 V
Average value: 586 V Grade Count:61
Hot Wire Ignition, HWI 7.00 - 59.0 sec
7.00 - 59.0 sec
Average value: 14.8 sec Grade Count:14
High Amp Arc Ignition, HAI 120 arcs
120 arcs
Average value: 120 arcs Grade Count:14
Users viewing this material also viewed the following: