Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 612, Impact Modified". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.00 - 1.07 g/cc
0.0361 - 0.0387 lb/in³
Average value: 1.03 g/cc Grade Count:7
0.820 - 0.820 g/cc

@Temperature 240 - 240 °C
0.0296 - 0.0296 lb/in³

@Temperature 464 - 464 °F
Average value: 0.820 g/cc Grade Count:1
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 27.0 - 33.0 MPa
3920 - 4790 psi
Average value: 29.0 MPa Grade Count:3
Tensile Strength, Yield 9.00 - 33.0 MPa
1310 - 4790 psi
Average value: 26.5 MPa Grade Count:6
Elongation at Break 41.0 - 300 %
41.0 - 300 %
Average value: 105 % Grade Count:7
Elongation at Yield 12.0 - 32.0 %
12.0 - 32.0 %
Average value: 25.7 % Grade Count:4
Modulus of Elasticity 0.720 - 1.19 GPa
104 - 172 ksi
Average value: 0.936 GPa Grade Count:3
0.0810 - 2.228 GPa

@Temperature -40.0 - 150 °C
11.7 - 323.1 ksi

@Temperature -40.0 - 302 °F
Average value: 0.954 GPa Grade Count:2
Flexural Yield Strength 23.0 - 52.0 MPa
3340 - 7540 psi
Average value: 33.7 MPa Grade Count:3
Flexural Modulus 0.520 - 1.30 GPa
75.4 - 189 ksi
Average value: 0.850 GPa Grade Count:5
Izod Impact, Notched 0.290 - 0.850 J/cm
0.543 - 1.59 ft-lb/in
Average value: 0.647 J/cm Grade Count:3
Izod Impact, Notched (ISO) 13.0 - 13.0 kJ/m²

@Temperature -30.0 - -30.0 °C
6.19 - 6.19 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 13.0 kJ/m² Grade Count:1
Charpy Impact, Notched 3.50 - 8.00 J/cm²
16.7 - 38.1 ft-lb/in²
Average value: 6.10 J/cm² Grade Count:3
1.20 - 1.50 J/cm²

@Temperature -30.0 - -30.0 °C
5.71 - 7.14 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 1.38 J/cm² Grade Count:2
Thermal Properties Metric English Comments
Melting Point 135 - 218 °C
275 - 424 °F
Average value: 193 °C Grade Count:7
Deflection Temperature at 0.46 MPa (66 psi) 60.0 - 151 °C
140 - 304 °F
Average value: 99.8 °C Grade Count:5
Deflection Temperature at 1.8 MPa (264 psi) 45.0 - 98.0 °C
113 - 208 °F
Average value: 56.2 °C Grade Count:5
Processing Properties Metric English Comments
Melt Temperature 230 - 250 °C
446 - 482 °F
Average value: 240 °C Grade Count:3
Drying Temperature 75.0 - 80.0 °C
167 - 176 °F
Average value: 77.5 °C Grade Count:3
Moisture Content 0.0600 %
0.0600 %
Average value: 0.0600 % Grade Count:3