Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 6, Unreinforced, Flame Retardant

Category Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, Unreinforced, Flame Retardant
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 6, Unreinforced, Flame Retardant.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Unreinforced, Flame Retardant". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.932 - 1.64 g/cc
0.0337 - 0.0592 lb/in³
Average value: 1.19 g/cc Grade Count:114
Water Absorption 0.0600 - 9.50 %
0.0600 - 9.50 %
Average value: 3.53 % Grade Count:55
Moisture Absorption at Equilibrium 0.170 - 3.50 %
0.170 - 3.50 %
Average value: 2.28 % Grade Count:40
Viscosity 2.60 cP
2.60 cP
Average value: 2.60 cP Grade Count:12
Linear Mold Shrinkage 0.000400 - 0.0190 cm/cm
0.000400 - 0.0190 in/in
Average value: 0.0116 cm/cm Grade Count:93
Linear Mold Shrinkage, Transverse 0.000400 - 0.0160 cm/cm
0.000400 - 0.0160 in/in
Average value: 0.0103 cm/cm Grade Count:35
Melt Flow 8.00 - 160 g/10 min
8.00 - 160 g/10 min
Average value: 39.9 g/10 min Grade Count:22
Mechanical Properties Metric English Comments
Hardness, Rockwell R 97.0 - 122
97.0 - 122
Average value: 114 Grade Count:39
Hardness, Shore D 71.0 - 83.0
71.0 - 83.0
Average value: 76.8 Grade Count:6
Ball Indentation Hardness 70.0 - 150 MPa
10200 - 21800 psi
Average value: 112 MPa Grade Count:3
Tensile Strength, Ultimate 17.0 - 148 MPa
2470 - 21500 psi
Average value: 70.8 MPa Grade Count:72
20.0 - 130 MPa

@Temperature -40.0 - 120 °C
2900 - 18900 psi

@Temperature -40.0 - 248 °F
Average value: 58.7 MPa Grade Count:11
Tensile Strength, Yield 35.0 - 90.0 MPa
5080 - 13100 psi
Average value: 65.7 MPa Grade Count:54
20.0 - 142 MPa

@Temperature -40.0 - 120 °C
2900 - 20600 psi

@Temperature -40.0 - 248 °F
Average value: 62.5 MPa Grade Count:8
Elongation at Break 2.00 - 200 %
2.00 - 200 %
Average value: 33.8 % Grade Count:102
2.50 - 70.0 %

@Temperature -40.0 - 150 °C
2.50 - 70.0 %

@Temperature -40.0 - 302 °F
Average value: 61.2 % Grade Count:8
Elongation at Yield 3.00 - 30.0 %
3.00 - 30.0 %
Average value: 9.18 % Grade Count:38
3.00 - 42.0 %

@Temperature -40.0 - 120 °C
3.00 - 42.0 %

@Temperature -40.0 - 248 °F
Average value: 26.6 % Grade Count:8
Modulus of Elasticity 0.970 - 10.8 GPa
141 - 1570 ksi
Average value: 3.09 GPa Grade Count:72
0.320 - 4.09 GPa

@Temperature -40.0 - 150 °C
46.4 - 593 ksi

@Temperature -40.0 - 302 °F
Average value: 1.17 GPa Grade Count:8
Flexural Yield Strength 25.0 - 360 MPa
3630 - 52200 psi
Average value: 94.7 MPa Grade Count:85
17.0 - 183 MPa

@Temperature -40.0 - 120 °C
2470 - 26500 psi

@Temperature -40.0 - 248 °F
Average value: 85.1 MPa Grade Count:12
Flexural Modulus 0.600 - 9.20 GPa
87.0 - 1330 ksi
Average value: 2.60 GPa Grade Count:88
0.305 - 5.50 GPa

@Temperature -40.0 - 120 °C
44.2 - 798 ksi

@Temperature -40.0 - 248 °F
Average value: 1.40 GPa Grade Count:8
Compressive Yield Strength 62.0 - 85.0 MPa
8990 - 12300 psi
Average value: 74.2 MPa Grade Count:5
Izod Impact, Notched 0.300 J/cm - NB
0.562 ft-lb/in - NB
Average value: 1.04 J/cm Grade Count:46
0.210 - 0.500 J/cm

@Temperature -40.0 - -40.0 °C
0.393 - 0.937 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 0.374 J/cm Grade Count:11
Izod Impact, Unnotched 4.81 - 5340 J/cm
9.00 - 10000 ft-lb/in
Average value: 7.74 J/cm Grade Count:6
Izod Impact, Notched (ISO) 3.00 - 10.0 kJ/m²
1.43 - 4.76 ft-lb/in²
Average value: 5.65 kJ/m² Grade Count:21
3.00 - 10.0 kJ/m²

@Temperature -40.0 - -20.0 °C
1.43 - 4.76 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 5.09 kJ/m² Grade Count:9
Izod Impact, Unnotched (ISO) 50.0 - 120 kJ/m²
23.8 - 57.1 ft-lb/in²
Average value: 89.0 kJ/m² Grade Count:5
100 - 100 kJ/m²

@Temperature -30.0 - -30.0 °C
47.6 - 47.6 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 100 kJ/m² Grade Count:1
Charpy Impact Unnotched 0.400 J/cm² - NB
1.90 ft-lb/in² - NB
Average value: 7.75 J/cm² Grade Count:49
5.00 - 999.9 J/cm²

@Temperature -30.0 - -20.0 °C
23.8 - 4759 ft-lb/in²

@Temperature -22.0 - -4.00 °F
Average value: 9.26 J/cm² Grade Count:23
Charpy Impact, Notched 0.200 - 5.50 J/cm²
0.952 - 26.2 ft-lb/in²
Average value: 0.635 J/cm² Grade Count:54
0.200 - 1.00 J/cm²

@Temperature -30.0 - -20.0 °C
0.952 - 4.76 ft-lb/in²

@Temperature -22.0 - -4.00 °F
Average value: 0.354 J/cm² Grade Count:26
Thermal Properties Metric English Comments
CTE, linear 30.0 - 100 µm/m-°C
16.7 - 55.6 µin/in-°F
Average value: 73.7 µm/m-°C Grade Count:34
CTE, linear, Transverse to Flow 78.0 - 190 µm/m-°C
43.3 - 106 µin/in-°F
Average value: 108 µm/m-°C Grade Count:6
Specific Heat Capacity 3.73 J/g-°C
0.891 BTU/lb-°F
Average value: 3.73 J/g-°C Grade Count:4
Thermal Conductivity 0.230 - 0.290 W/m-K
1.60 - 2.01 BTU-in/hr-ft²-°F
Average value: 0.263 W/m-K Grade Count:6
Melting Point 215 - 265 °C
419 - 509 °F
Average value: 221 °C Grade Count:67
Maximum Service Temperature, Air 90.0 - 180 °C
194 - 356 °F
Average value: 117 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 140 - 240 °C
284 - 464 °F
Average value: 184 °C Grade Count:58
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+8 - 1.00e+17 ohm-cm
1.00e+8 - 1.00e+17 ohm-cm
Average value: 1.90e+15 ohm-cm Grade Count:64
Surface Resistance 1.00e+10 - 1.00e+16 ohm
1.00e+10 - 1.00e+16 ohm
Average value: 5.72e+14 ohm Grade Count:40
Dielectric Constant 3.00 - 8.00
3.00 - 8.00
Average value: 4.13 Grade Count:22
Dielectric Strength 12.0 - 100 kV/mm
305 - 2540 kV/in
Average value: 25.1 kV/mm Grade Count:53
Dissipation Factor 0.00780 - 0.125
0.00780 - 0.125
Average value: 0.0316 Grade Count:15
Arc Resistance 60.0 - 179 sec
60.0 - 179 sec
Average value: 115 sec Grade Count:7
Comparative Tracking Index 250 - 600 V
250 - 600 V
Average value: 556 V Grade Count:55
Hot Wire Ignition, HWI 7.00 - 60.0 sec
7.00 - 60.0 sec
Average value: 20.9 sec Grade Count:3
High Amp Arc Ignition, HAI 30.0 - 120 arcs
30.0 - 120 arcs
Average value: 105 arcs Grade Count:3