Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Glass Bead Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.920 - 1.66 g/cc
0.0332 - 0.0600 lb/in³
Average value: 1.35 g/cc Grade Count:109
Filler Content 10.0 - 40.0 %
10.0 - 40.0 %
Average value: 26.7 % Grade Count:6
Water Absorption 0.800 - 8.00 %
0.800 - 8.00 %
Average value: 2.53 % Grade Count:39
Moisture Absorption at Equilibrium 0.250 - 3.00 %
0.250 - 3.00 %
Average value: 1.94 % Grade Count:33
Water Absorption at Saturation 5.80 - 7.30 %
5.80 - 7.30 %
Average value: 6.54 % Grade Count:10
Viscosity Test 140 - 150 cm³/g
140 - 150 cm³/g
Average value: 145 cm³/g Grade Count:4
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cm
0.00100 - 0.0200 in/in
Average value: 0.00906 cm/cm Grade Count:95
Linear Mold Shrinkage, Transverse 0.00200 - 0.100 cm/cm
0.00200 - 0.100 in/in
Average value: 0.0150 cm/cm Grade Count:30
Melt Flow 3.00 - 115 g/10 min
3.00 - 115 g/10 min
Average value: 39.2 g/10 min Grade Count:21
Mechanical Properties Metric English Comments
Hardness, Rockwell R 110 - 122
110 - 122
Average value: 118 Grade Count:13
Hardness, Shore D 80.0 - 90.0
80.0 - 90.0
Average value: 85.4 Grade Count:4
Ball Indentation Hardness 75.0 - 220 MPa
10900 - 31900 psi
Average value: 148 MPa Grade Count:10
Tensile Strength, Ultimate 30.0 - 147 MPa
4350 - 21300 psi
Average value: 73.2 MPa Grade Count:90
20.0 - 45.0 MPa

@Temperature 60.0 - 150 °C
2900 - 6530 psi

@Temperature 140 - 302 °F
Average value: 31.3 MPa Grade Count:1
Tensile Strength, Yield 35.0 - 121 MPa
5080 - 17500 psi
Average value: 81.1 MPa Grade Count:24
Elongation at Break 0.500 - 155 %
0.500 - 155 %
Average value: 9.54 % Grade Count:100
10.0 - 35.0 %

@Temperature 60.0 - 150 °C
10.0 - 35.0 %

@Temperature 140 - 302 °F
Average value: 20.0 % Grade Count:1
Elongation at Yield 2.70 - 15.0 %
2.70 - 15.0 %
Average value: 7.30 % Grade Count:13
8.00 - 14.0 %

@Temperature 60.0 - 150 °C
8.00 - 14.0 %

@Temperature 140 - 302 °F
Average value: 11.5 % Grade Count:1
Modulus of Elasticity 1.35 - 8.96 GPa
196 - 1300 ksi
Average value: 4.18 GPa Grade Count:87
0.580 - 2.00 GPa

@Temperature 60.0 - 150 °C
84.1 - 290 ksi

@Temperature 140 - 302 °F
Average value: 1.10 GPa Grade Count:1
Flexural Yield Strength 10.3 - 230 MPa
1500 - 33400 psi
Average value: 123 MPa Grade Count:74
Flexural Modulus 1.57 - 8.62 GPa
228 - 1250 ksi
Average value: 4.38 GPa Grade Count:83
Izod Impact, Notched 0.160 - 1.28 J/cm
0.300 - 2.40 ft-lb/in
Average value: 0.506 J/cm Grade Count:27
Izod Impact, Unnotched 1.33 J/cm - NB
2.50 ft-lb/in - NB
Average value: 5.25 J/cm Grade Count:21
Izod Impact, Notched (ISO) 2.50 - 12.0 kJ/m²
1.19 - 5.71 ft-lb/in²
Average value: 5.29 kJ/m² Grade Count:33
2.00 - 42.0 kJ/m²

@Temperature -40.0 - -30.0 °C
0.952 - 20.0 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 10.8 kJ/m² Grade Count:8
Izod Impact, Unnotched (ISO) 15.0 - 80.0 kJ/m²
7.14 - 38.1 ft-lb/in²
Average value: 34.0 kJ/m² Grade Count:18
25.0 - 40.0 kJ/m²

@Temperature -30.0 - -30.0 °C
11.9 - 19.0 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 34.7 kJ/m² Grade Count:5
Charpy Impact Unnotched 1.50 J/cm² - NB
7.14 ft-lb/in² - NB
Average value: 4.90 J/cm² Grade Count:59
2.00 - 9.00 J/cm²

@Temperature -30.0 - 30.0 °C
9.52 - 42.8 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 4.20 J/cm² Grade Count:26
Charpy Impact, Notched 0.200 - 1.80 J/cm²
0.952 - 8.57 ft-lb/in²
Average value: 0.668 J/cm² Grade Count:57
0.100 - 1.00 J/cm²

@Temperature -40.0 - 30.0 °C
0.476 - 4.76 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 0.476 J/cm² Grade Count:23
Puncture Energy 1.70 - 1.70 J

@Temperature -30.0 - -30.0 °C
1.25 - 1.25 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 1.70 J Grade Count:2
1.70 - 1.70 J

@Load <=70.4 kg
1.25 - 1.25 ft-lb

@Load <=155 lb
Average value: 1.70 J Grade Count:2
Tensile Creep Modulus, 1000 hours 2000 MPa
290000 psi
Average value: 2000 MPa Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 17.1 - 90.0 µm/m-°C
9.50 - 50.0 µin/in-°F
Average value: 48.4 µm/m-°C Grade Count:38
CTE, linear, Transverse to Flow 60.0 - 118 µm/m-°C
33.3 - 65.6 µin/in-°F
Average value: 86.3 µm/m-°C Grade Count:17
Specific Heat Capacity 1.40 J/g-°C
0.335 BTU/lb-°F
Average value: 1.40 J/g-°C Grade Count:4
Thermal Conductivity 0.340 - 0.360 W/m-K
2.36 - 2.50 BTU-in/hr-ft²-°F
Average value: 0.344 W/m-K Grade Count:5
Melting Point 205 - 255 °C
401 - 491 °F
Average value: 220 °C Grade Count:67
Maximum Service Temperature, Air 80.0 - 200 °C
176 - 392 °F
Average value: 140 °C Grade Count:10
Deflection Temperature at 0.46 MPa (66 psi) 170 - 218 °C
338 - 424 °F
Average value: 197 °C Grade Count:53
Deflection Temperature at 1.8 MPa (264 psi) 50.0 - 230 °C
122 - 446 °F
Average value: 127 °C Grade Count:89
Vicat Softening Point 190 - 247 °C
374 - 477 °F
Average value: 204 °C Grade Count:33
Flammability, UL94 HB - V-0
HB - V-0
Grade Count:70
Oxygen Index 24.0 - 31.0 %
24.0 - 31.0 %
Average value: 27.3 % Grade Count:4
Glow Wire Test 390 - 960 °C
734 - 1760 °F
Average value: 685 °C Grade Count:19
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+10 - 1.00e+15 ohm-cm
1.00e+10 - 1.00e+15 ohm-cm
Average value: 4.78e+14 ohm-cm Grade Count:48
Surface Resistance 1.00e+10 - 1.00e+16 ohm
1.00e+10 - 1.00e+16 ohm
Average value: 7.47e+14 ohm Grade Count:31
Dielectric Constant 2.60 - 6.00
2.60 - 6.00
Average value: 4.55 Grade Count:25
Dielectric Strength 15.7 - 80.0 kV/mm
400 - 2030 kV/in
Average value: 33.2 kV/mm Grade Count:35
Dissipation Factor 0.0180 - 0.0700
0.0180 - 0.0700
Average value: 0.0371 Grade Count:7
Dielectric Loss Index 0.0200 - 0.200
0.0200 - 0.200
Average value: 0.110 Grade Count:16
Comparative Tracking Index 250 - 600 V
250 - 600 V
Average value: 456 V Grade Count:30