Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6-3". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.08 - 1.65 g/cc
0.0390 - 0.0596 lb/in³
Average value: 1.32 g/cc Grade Count:14
Water Absorption 5.50 - 8.00 %
5.50 - 8.00 %
Average value: 7.17 % Grade Count:6
Moisture Absorption at Equilibrium 1.50 - 2.10 %
1.50 - 2.10 %
Average value: 1.90 % Grade Count:6
Viscosity Test 115 - 160 cm³/g
115 - 160 cm³/g
Average value: 131 cm³/g Grade Count:6
Linear Mold Shrinkage 0.00100 - 0.00400 cm/cm
0.00100 - 0.00400 in/in
Average value: 0.00333 cm/cm Grade Count:6
Linear Mold Shrinkage, Transverse 0.00600 - 0.00900 cm/cm
0.00600 - 0.00900 in/in
Average value: 0.00817 cm/cm Grade Count:6
Mechanical Properties Metric English Comments
Hardness, Shore D 84.0 - 90.0
84.0 - 90.0
Average value: 87.3 Grade Count:8
Ball Indentation Hardness 130 - 310 MPa
18900 - 45000 psi
Average value: 195 MPa Grade Count:8
Tensile Strength, Ultimate 120 - 220 MPa
17400 - 31900 psi
Average value: 175 MPa Grade Count:9
Tensile Strength, Yield 82.0 - 90.0 MPa
11900 - 13100 psi
Average value: 88.0 MPa Grade Count:5
Elongation at Break 2.00 - 50.0 %
2.00 - 50.0 %
Average value: 19.1 % Grade Count:14
Elongation at Yield 6.00 - 9.00 %
6.00 - 9.00 %
Average value: 8.10 % Grade Count:5
Modulus of Elasticity 2.20 - 14.5 GPa
319 - 2100 ksi
Average value: 7.24 GPa Grade Count:14
Flexural Yield Strength 80.0 - 342 MPa
11600 - 49600 psi
Average value: 153 MPa Grade Count:6
Flexural Modulus 2.70 - 12.0 GPa
392 - 1740 ksi
Average value: 4.45 GPa Grade Count:6
Izod Impact, Unnotched (ISO) 9.50 - 9.50 kJ/m²

@Temperature -40.0 - -40.0 °C
4.52 - 4.52 ft-lb/in²

@Temperature -40.0 - -40.0 °F
Average value: 9.50 kJ/m² Grade Count:1
Charpy Impact Unnotched 6.00 J/cm² - NB
28.6 ft-lb/in² - NB
Average value: 8.73 J/cm² Grade Count:14
5.00 J/cm² - NB

@Temperature -30.0 - 0.000 °C
23.8 ft-lb/in² - NB

@Temperature -22.0 - 32.0 °F
Average value: 6.93 J/cm² Grade Count:14
Charpy Impact, Notched 0.900 - 2.10 J/cm²
4.28 - 9.99 ft-lb/in²
Average value: 1.32 J/cm² Grade Count:14
0.600 - 1.10 J/cm²

@Temperature -30.0 - 0.000 °C
2.86 - 5.24 ft-lb/in²

@Temperature -22.0 - 32.0 °F
Average value: 0.902 J/cm² Grade Count:14
Tensile Creep Modulus, 1 hour 2200 - 9600 MPa
319000 - 1.39e+6 psi
Average value: 3550 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 800 - 5200 MPa
116000 - 754000 psi
Average value: 1880 MPa Grade Count:6
Thermal Properties Metric English Comments
CTE, linear 20.0 - 70.0 µm/m-°C
11.1 - 38.9 µin/in-°F
Average value: 40.2 µm/m-°C Grade Count:10
CTE, linear, Transverse to Flow 20.0 - 70.0 µm/m-°C
11.1 - 38.9 µin/in-°F
Average value: 52.9 µm/m-°C Grade Count:11
Melting Point 260 °C
500 °F
Average value: 260 °C Grade Count:7
Deflection Temperature at 0.46 MPa (66 psi) 85.0 - 260 °C
185 - 500 °F
Average value: 192 °C Grade Count:11
Deflection Temperature at 1.8 MPa (264 psi) 75.0 - 255 °C
167 - 491 °F
Average value: 176 °C Grade Count:10
Vicat Softening Point 99.0 - 230 °C
210 - 446 °F
Average value: 174 °C Grade Count:8
Glass Transition Temp, Tg 93.0 - 153 °C
199 - 307 °F
Average value: 131 °C Grade Count:6
UL RTI, Mechanical with Impact 65.0 - 80.0 °C
149 - 176 °F
Average value: 72.5 °C Grade Count:3
UL RTI, Mechanical without Impact 65.0 - 85.0 °C
149 - 185 °F
Average value: 75.0 °C Grade Count:3
Flammability, UL94 HB - V-2
HB - V-2
Grade Count:8
Glow Wire Test 850 °C
1560 °F
Average value: 850 °C Grade Count:3
Optical Properties Metric English Comments
Transmission, Visible 90.0 %
90.0 %
Average value: 90.0 % Grade Count:4
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+12 - 1.00e+15 ohm-cm
1.00e+12 - 1.00e+15 ohm-cm
Average value: 5.25e+14 ohm-cm Grade Count:12
Surface Resistance 1.00e+13 - 1.00e+15 ohm
1.00e+13 - 1.00e+15 ohm
Average value: 4.06e+14 ohm Grade Count:9
Dielectric Constant 3.30 - 10.0
3.30 - 10.0
Average value: 4.81 Grade Count:11
Dielectric Strength 19.0 - 35.0 kV/mm
483 - 889 kV/in
Average value: 26.6 kV/mm Grade Count:12
Dissipation Factor 0.00500 - 0.300
0.00500 - 0.300
Average value: 0.0640 Grade Count:12
Comparative Tracking Index 500 - 600 V
500 - 600 V
Average value: 575 V Grade Count:8