Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 11, Cable Sheathing Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.03 - 1.11 g/cc
0.0372 - 0.0401 lb/in³
Average value: 1.06 g/cc Grade Count:8
Water Absorption 1.50 - 1.96 %
1.50 - 1.96 %
Average value: 1.74 % Grade Count:7
Melt Flow 27.5 - 95.1 g/10 min
27.5 - 95.1 g/10 min
Average value: 50.8 g/10 min Grade Count:6
Mechanical Properties Metric English Comments
Tensile Strength, Yield 25.0 - 56.0 MPa
3630 - 8120 psi
Average value: 39.7 MPa Grade Count:10
Elongation at Break 50.0 %
50.0 %
Average value: 50.0 % Grade Count:6
Elongation at Yield 5.00 - 10.0 %
5.00 - 10.0 %
Average value: 6.00 % Grade Count:6
Modulus of Elasticity 0.330 - 2.07 GPa
47.9 - 300 ksi
Average value: 1.22 GPa Grade Count:10
Charpy Impact Unnotched 1000 J/cm² - NB
4760 ft-lb/in² - NB
Grade Count:4
0.850 - 999.9 J/cm²

@Temperature -30.0 - -30.0 °C
4.05 - 4759 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 0.850 J/cm² Grade Count:3
Charpy Impact, Notched 0.420 - 1000 J/cm²
2.00 - 4760 ft-lb/in²
Average value: 0.770 J/cm² Grade Count:5
0.420 - 1.06 J/cm²

@Temperature -30.0 - -30.0 °C
2.00 - 5.04 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 0.712 J/cm² Grade Count:5
Thermal Properties Metric English Comments
CTE, linear 90.0 - 102 µm/m-°C
50.0 - 56.7 µin/in-°F
Average value: 97.3 µm/m-°C Grade Count:3
Melting Point 182 - 187 °C
360 - 369 °F
Average value: 184 °C Grade Count:8
Deflection Temperature at 1.8 MPa (264 psi) 45.0 - 55.0 °C
113 - 131 °F
Average value: 49.8 °C Grade Count:4
Flammability, UL94 HB - V-0
HB - V-0
Grade Count:8
Oxygen Index 25.0 - 33.0 %
25.0 - 33.0 %
Average value: 29.3 % Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+12 - 1.00e+15 ohm-cm
1.00e+12 - 1.00e+15 ohm-cm
Average value: 3.00e+14 ohm-cm Grade Count:4
Surface Resistance 1.00e+14 - 1.00e+15 ohm
1.00e+14 - 1.00e+15 ohm
Average value: 4.00e+14 ohm Grade Count:3
Dielectric Strength 20.0 - 30.0 kV/mm
508 - 762 kV/in
Average value: 26.2 kV/mm Grade Count:3
Dissipation Factor 0.000306 - 0.000330
0.000306 - 0.000330
Average value: 0.000320 Grade Count:3
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:3
Processing Properties Metric English Comments
Melt Temperature 190 - 250 °C
374 - 482 °F
Average value: 220 °C Grade Count:4
Drying Temperature 80.0 - 90.0 °C
176 - 194 °F
Average value: 85.0 °C Grade Count:4
Moisture Content 0.100 %
0.100 %
Average value: 0.100 % Grade Count:4