Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acrylic, Cast". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.18 - 1.19 g/cc
0.0426 - 0.0430 lb/in³
Average value: 1.19 g/cc Grade Count:10
Water Absorption 0.130 - 0.480 %
0.130 - 0.480 %
Average value: 0.296 % Grade Count:8
Water Absorption at Saturation 1.10 - 2.10 %
1.10 - 2.10 %
Average value: 1.90 % Grade Count:5
Moisture Expansion 0.500 %
0.500 %
Average value: 0.500 % Grade Count:3
Moisture Vapor Transmission 55.0 cc-mm/m²-24hr-atm
140 cc-mil/100 in²-24hr-atm
Average value: 55.0 cc-mm/m²-24hr-atm Grade Count:3
Mechanical Properties Metric English Comments
Hardness, Rockwell M 94.0 - 102
94.0 - 102
Average value: 98.2 Grade Count:3
Ball Indentation Hardness 175 MPa
25400 psi
Average value: 175 MPa Grade Count:3
Tensile Strength, Ultimate 62.0 - 83.0 MPa
8990 - 12000 psi
Average value: 77.0 MPa Grade Count:10
40.0 - 110 MPa

@Temperature -40.0 - 70.0 °C
5800 - 16000 psi

@Temperature -40.0 - 158 °F
Average value: 75.0 MPa Grade Count:3
Elongation at Break 4.00 - 5.50 %
4.00 - 5.50 %
Average value: 5.02 % Grade Count:9
Modulus of Elasticity 2.80 - 3.30 GPa
406 - 479 ksi
Average value: 3.17 GPa Grade Count:4
Flexural Yield Strength 105 - 116 MPa
15200 - 16800 psi
Average value: 113 MPa Grade Count:6
Flexural Modulus 2.96 - 3.30 GPa
429 - 479 ksi
Average value: 3.16 GPa Grade Count:3
Compressive Yield Strength 110 - 124 MPa
16000 - 18000 psi
Average value: 114 MPa Grade Count:4
Poissons Ratio 0.370
0.370
Average value: 0.370 Grade Count:3
Shear Modulus 1.70 GPa
247 ksi
Average value: 1.70 GPa Grade Count:3
Izod Impact, Notched (ISO) 1.60 kJ/m²
0.761 ft-lb/in²
Average value: 1.60 kJ/m² Grade Count:3
Charpy Impact Unnotched 1.20 - 2.17 J/cm²
5.71 - 10.3 ft-lb/in²
Average value: 1.57 J/cm² Grade Count:5
Coefficient of Friction 0.450 - 0.800
0.450 - 0.800
Average value: 0.583 Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 61.0 - 104 µm/m-°C
33.9 - 57.8 µin/in-°F
Average value: 74.0 µm/m-°C Grade Count:8
Specific Heat Capacity 1.47 J/g-°C
0.351 BTU/lb-°F
Average value: 1.47 J/g-°C Grade Count:6
Thermal Conductivity 0.190 W/m-K
1.32 BTU-in/hr-ft²-°F
Average value: 0.190 W/m-K Grade Count:6
Maximum Service Temperature, Air 80.0 - 200 °C
176 - 392 °F
Average value: 123 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 113 - 115 °C
235 - 239 °F
Average value: 114 °C Grade Count:3
Deflection Temperature at 1.8 MPa (264 psi) 99.0 - 112 °C
210 - 234 °F
Average value: 106 °C Grade Count:6
Vicat Softening Point 105 - 118 °C
221 - 244 °F
Average value: 113 °C Grade Count:8
Flash Point 425 °C
797 °F
Average value: 425 °C Grade Count:3
Optical Properties Metric English Comments
Refractive Index 1.49 - 1.49
1.49 - 1.49
Average value: 1.49 Grade Count:7
Haze 0.500 - 2.20 %
0.500 - 2.20 %
Average value: 1.06 % Grade Count:5
Transmission, Visible 89.0 - 92.0 %
89.0 - 92.0 %
Average value: 91.3 % Grade Count:9
UV Transmittance 0.000 - 1.00 %
0.000 - 1.00 %
Average value: 0.400 % Grade Count:5
Reflection Coefficient, Visible (0-1) 0.0400
0.0400
Average value: 0.0400 Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+15 - 1.60e+16 ohm-cm
1.00e+15 - 1.60e+16 ohm-cm
Average value: 4.75e+15 ohm-cm Grade Count:4
Surface Resistance 5.00e+13 - 1.90e+15 ohm
5.00e+13 - 1.90e+15 ohm
Average value: 5.12e+14 ohm Grade Count:4
Shielding Effectiveness 26.0 - 32.0 dB
26.0 - 32.0 dB
Average value: 29.3 dB Grade Count:3
Dielectric Constant 2.70 - 3.60
2.70 - 3.60
Average value: 3.14 Grade Count:4
Dielectric Strength 17.0 - 30.0 kV/mm
432 - 762 kV/in
Average value: 26.8 kV/mm Grade Count:4
Dissipation Factor 0.0200 - 0.0600
0.0200 - 0.0600
Average value: 0.0400 Grade Count:4
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:3
Processing Properties Metric English Comments
Processing Temperature 80.0 - 193 °C
176 - 379 °F
Average value: 134 °C Grade Count:4