Material Notes:
Fairly good corrosion resistant formable steel in mildly corrosive environments. Oxidation resistant at elevated temperatures (up to ~800°C). Ductile, does not work harden readily, and is well suited for deep drawing and bending.Applications: Used in a variety of interior applications where material cost and corrosion performance are important factors. Typical applications include: Washing machinesDish-washersSinksElectrical tie-wireVine wireSink rimsCounter topsCooker hoodsRefrigeratorsTablewareRestaurant equipmentIndoor claddingFlue-gas ductsAvailable in cold rolled narrow strip, bar, and rod forms.
Physical Properties Metric English Comments
Density 7.70 g/cc
0.278 lb/in³
RT
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 520 MPa
75400 psi
Outokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
Tensile Strength, Yield 260 MPa

@Strain 0.200 %
37700 psi

@Strain 0.200 %
EN min.,RT; EN 10002-1
380 MPa

@Strain 0.200 %
55100 psi

@Strain 0.200 %
Outokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
190 MPa

@Strain 0.200 %,
Temperature 400 °C
27600 psi

@Strain 0.200 %,
Temperature 752 °F
EN min.; EN 10002-5
200 MPa

@Strain 0.200 %,
Temperature 300 °C
29000 psi

@Strain 0.200 %,
Temperature 572 °F
EN min.; EN 10002-5
210 MPa

@Strain 0.200 %,
Temperature 200 °C
30500 psi

@Strain 0.200 %,
Temperature 392 °F
EN min.; EN 10002-5
220 MPa

@Strain 0.200 %,
Temperature 100 °C
31900 psi

@Strain 0.200 %,
Temperature 212 °F
EN min.; EN 10002-5
Elongation at Break 25 %
25 %
Outokumpu Typical, Cold Rolled Strip/Sheet; EN 10002-1
Modulus of Elasticity 220 GPa
31900 ksi
RT
195 GPa

@Temperature 400 °C
28300 ksi

@Temperature 752 °F
205 GPa

@Temperature 300 °C
29700 ksi

@Temperature 572 °F
210 GPa

@Temperature 200 °C
30500 ksi

@Temperature 392 °F
215 GPa

@Temperature 100 °C
31200 ksi

@Temperature 212 °F
Thermal Properties Metric English Comments
CTE, linear 10.0 µm/m-°C

@Temperature 100 °C
5.56 µin/in-°F

@Temperature 212 °F
10.5 µm/m-°C

@Temperature 300 °C
5.83 µin/in-°F

@Temperature 572 °F
10.5 µm/m-°C

@Temperature 400 °C
5.83 µin/in-°F

@Temperature 752 °F
11.0 µm/m-°C

@Temperature 500 °C
6.11 µin/in-°F

@Temperature 932 °F
Specific Heat Capacity 0.460 J/g-°C
0.110 BTU/lb-°F
RT
Thermal Conductivity 25.0 W/m-K
174 BTU-in/hr-ft²-°F
RT
25.0 W/m-K

@Temperature 400 °C
174 BTU-in/hr-ft²-°F

@Temperature 752 °F
Component Elements Properties Metric English Comments
Carbon, C 0.040 %
0.040 %
Chromium, Cr 16.5 %
16.5 %
Iron, Fe 83.46 %
83.46 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.0000600 ohm-cm
0.0000600 ohm-cm
RT