Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Noltex Soarnol® DT2903 Ethylene Vinyl Alcohol Copolymer

Category Polymer , Thermoplastic , Ethylene Vinyl Alcohol (EVOH)
Manufacturer Noltex
Trade Name Soarnol®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Noltex Soarnol® DT2903 Ethylene Vinyl Alcohol Copolymer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Very low ethylene content, high gas barrier for packaging dry products or for use in packaging material used at normal temperature and humidity. Ethylene content 29 mol%. Volatile matter 0.3%.The gas barrier property of Soarnol is about forty times better than that of nylon, therefore, Soarnol allows design of lower cost packages by using a thin gas barrier layer without loss of shelf life.Soarnol DT2903 with low melt flow index is one of the standard grade of Soarnol, its ethylene content is 29 mol%. Since Soarnol DT2903 has a good gas barrier at low humidity, this resin is suited for coextruded film and coextrusion coating. This resin can also be used in coextruded sheet, coextruded blow-molded containers and coextruded inflation film.Processing: Extruder:40 m screw type, L/D=28;Screw:Full-flighted, constant pitch type, CR=4.0;Screen pack:80/120/50 mesh;Die:Manifold type, die width=450 mm, lip distance=0.2 mm.Information provided by Soarus, LLC. In the United States SOARNOL is produced by Noltex,L.L.C., an affiliate of Nippon Gohsei.
Physical Properties Metric English Comments
Density 1.21 g/cc
0.0437 lb/in³
Moisture Vapor Transmission 1.11 - 2.10 cc-mm/m²-24hr-atm
2.82 - 5.33 cc-mil/100 in²-24hr-atm
40°C- 90% RH; based on 30 µm layer
Oxygen Transmission 0.00800 cc-mm/m²-24hr-atm
0.0203 cc-mil/100 in²-24hr-atm
20°C- 65% RH; based on 20 µm layer
Viscosity 800000 cP

@Shear Rate 250 1/s,
Temperature 230 °C
800000 cP

@Shear Rate 250 1/s,
Temperature 446 °F
Melt Flow 3.2 g/10 min

@Load 2.16 kg,
Temperature 210 °C
3.2 g/10 min

@Load 4.76 lb,
Temperature 410 °F
Thermal Properties Metric English Comments
Melting Point 188 °C
370 °F
DSC, both heating and cooling speeds of 20°C/min
Crystallization Temperature 163 °C
325 °F
DSC, both heating and cooling speeds of 20°C/min
Glass Transition Temp, Tg 62.0 °C
144 °F
DSC, both heating and cooling speeds of 20°C/min
Optical Properties Metric English Comments
Refractive Index 1.525
1.525
Quenched
1.534
1.534
Annealed at 140°C, 30 min
Processing Properties Metric English Comments
Nozzle Temperature 200 - 220 °C
392 - 428 °F
Users viewing this material also viewed the following: