Material Notes:
In addition to the excellent properties of Murytal® C, Murytal® H is stronger and more rigid with a lower expansion coefficient.Special Properties:• High rigidity• Excellent ability to regain its form• Extremely good electric isolation properties• Practically no moisture absorption• Good resistance to chemicals (pH 4 – 9) • Approved for use in the food industry (EU and FDA) • Extremely good machinabilityInformation provided by Murtfeldt Kunststoffe GmbH & Co. KG.
Physical Properties Metric English Comments
Density 1.43 g/cc
0.0517 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 0.20 %

@Temperature 23.0 °C
0.20 %

@Temperature 73.4 °F
50% RH
Water Absorption at Saturation 0.80 %

@Temperature 23.0 °C
0.80 %

@Temperature 73.4 °F
Mechanical Properties Metric English Comments
Hardness, Rockwell M 88
88
dry; ISO 2039-2
Hardness, Shore D 83
83
DIN 53505
Ball Indentation Hardness 160 MPa
23200 psi
dry; ISO 2039-1
Tensile Strength, Yield 78.0 MPa
11300 psi
dry; ISO 527-1
78.0 MPa
11300 psi
50% RH; ISO 527-1
Elongation at Break 50 %
50 %
dry; ISO 527-1
50 %
50 %
50% RH; ISO 527-1
Creep Strength 15.0 MPa

@Time 3.60e+6 sec
2180 psi

@Time 1000 hour
stress leading to 1% elongation; dry; ISO 899-1
15.0 MPa

@Time 3.60e+6 sec
2180 psi

@Time 1000 hour
stress leading to 1% elongation; 50% RH; ISO 899-1
Modulus of Elasticity 3.30 GPa
479 ksi
dry
3.30 GPa
479 ksi
50% RH
Compressive Yield Strength 22.0 MPa

@Strain 1.00 %
3190 psi

@Strain 1.00 %
dry; ISO 604
40.0 MPa

@Strain 2.00 %
5800 psi

@Strain 2.00 %
dry; ISO 604
75.0 MPa

@Strain 5.00 %
10900 psi

@Strain 5.00 %
dry; ISO 604
Charpy Impact Unnotched 20.0 J/cm²
95.2 ft-lb/in²
dry; ISO 179-1/1eU
>= 20.0 J/cm²
>= 95.2 ft-lb/in²
ISO 179
Charpy Impact, Notched 1.00 J/cm²
4.76 ft-lb/in²
dry; ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.34
0.34
Thermal Properties Metric English Comments
CTE, linear 95.0 µm/m-°C

@Temperature 23.0 - 60.0 °C
52.8 µin/in-°F

@Temperature 73.4 - 140 °F
110 µm/m-°C

@Temperature 23.0 - 100 °C
61.1 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.310 W/m-K
2.15 BTU-in/hr-ft²-°F
Melting Point 180 °C
356 °F
ISO 11357-1
Maximum Service Temperature, Air 90.0 °C

@Time 7.20e+7 sec
194 °F

@Time 20000 hour
105 °C

@Time 1.80e+7 sec
221 °F

@Time 5000 hour
150 °C

@Time <=86400 sec
302 °F

@Time <=24.0 hour
Minimum Service Temperature, Air -50.0 °C
-58.0 °F
Glass Transition Temp, Tg -50.0 °C
-58.0 °F
ISO 11357-1
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Electrical Resistivity >= 1.00e+14 ohm-cm
>= 1.00e+14 ohm-cm
dry; IEC 60093
>= 1.00e+14 ohm-cm
>= 1.00e+14 ohm-cm
50% RH; IEC 60093
Surface Resistance >= 1.00e+13 ohm
>= 1.00e+13 ohm
dry; IEC 60093
>= 1.00e+13 ohm
>= 1.00e+13 ohm
50% RH; IEC 60093
Dielectric Constant 3.8

@Frequency 100 Hz
3.8

@Frequency 100 Hz
dry; IEC 60250
3.8

@Frequency 100 Hz
3.8

@Frequency 100 Hz
50% RH; IEC 60250
3.8

@Frequency 1.00e+6 Hz
3.8

@Frequency 1.00e+6 Hz
dry; IEC 60250
3.8

@Frequency 1.00e+6 Hz
3.8

@Frequency 1.00e+6 Hz
50% RH; IEC 60250
Dielectric Strength 20.0 kV/mm
508 kV/in
dry; IEC 60243-1
20.0 kV/mm
508 kV/in
50% RH; IEC 60243-1
Dielectric Loss Index 0.0030

@Frequency 100 Hz
0.0030

@Frequency 100 Hz
dry; IEC 60250
0.0030

@Frequency 100 Hz
0.0030

@Frequency 100 Hz
50% RH; IEC 60250
0.0080

@Frequency 1.00e+6 Hz
0.0080

@Frequency 1.00e+6 Hz
dry; IEC 60250
0.0080

@Frequency 1.00e+6 Hz
0.0080

@Frequency 1.00e+6 Hz
50% RH; IEC 60250
Compliance Properties Metric English Comments
FDA Yes
Yes
Descriptive Properties Value Comments
Color Natural/Black
Copyright © lookpolymers.com All Rights Reserved