Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Lucite International Perspexâ„¢ XT IM50 Acrylic Extruded Sheet

Category Polymer , Thermoplastic , Acrylic (PMMA) , Acrylic, Extruded
Manufacturer Lucite International
Trade Name Perspex™
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Lucite International Perspexâ„¢ XT IM50 Acrylic Extruded Sheet.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
PERSPEX extruded sheet has a lower molecular weight making it easy to vacuum form and the extrusion process gives excellent thickness tolerance and is economical for long production runs.Information provided by Lucite International.
Physical Properties Metric English Comments
Density 1.17 g/cc
0.0423 lb/in³
ISO 1183
Mechanical Properties Metric English Comments
Hardness, Rockwell M 65
65
ISO 2039-2
Tensile Strength, Ultimate 68.0 MPa
9860 psi
5 mm/min; ISO 527
Elongation at Break 18 %
18 %
5 mm/min; ISO 527
Flexural Strength 90.0 MPa
13100 psi
2 mm/min; ISO 178
Flexural Modulus 2.50 GPa
363 ksi
2 mm/min; ISO 178
Izod Impact, Notched (ISO) 5.00 kJ/m²
2.38 ft-lb/in²
ISO 180/1A
Charpy Impact Unnotched 5.00 J/cm²
23.8 ft-lb/in²
ISO 179
Charpy Impact, Notched 0.500 J/cm²
2.38 ft-lb/in²
ISO 179
Thermal Properties Metric English Comments
Vicat Softening Point >= 105 °C
>= 221 °F
ISO 306A
Flammability, UL94 HB
HB
Copyright © lookpolymers.com All Rights Reserved