Lubrizol Estane® S198A Thermoplastic Polyurethane

Category Polymer , Thermoplastic , Polyurethane, TP , Thermoplastic Polyurethane (TPUR), Polyester Grade
Manufacturer Lubrizol (former Noveon)
Trade Name ESTANE®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Lubrizol Estane® S198A Thermoplastic Polyurethane.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Type: Estane® S198A is a Shore 98A, polyester grade thermoplastic polyurethane (TPU). FDA approved (21 CFR 177.2600, 177.1680).Uses: Injection Molding.Availability: Americas, Europe, Middle East, Africa, India and AsiaInformation Provided by The Lubrizol Corporation
Physical Properties Metric English Comments
Specific Gravity 1.23 g/cc
1.23 g/cc
ASTM D792
Linear Mold Shrinkage 0.0080 cm/cm
0.0080 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Shore A 98
98
ASTM D2240
Hardness, Shore D 55
55
ASTM D2240
Tensile Strength, Ultimate 49.0 MPa
7110 psi
ASTM D412
Tensile Strength, Yield 15.7 MPa
2280 psi
at 100% elongation; ASTM D412
29.4 MPa
4270 psi
at 300% elongation; ASTM D412
Elongation at Break 520 %
520 %
ASTM D412
Tear Strength 177 kN/m
1010 pli
Die C; ASTM D624
Abrasion 25
25
mm<sup>3</sup> loss; ISO 4649
Compression Set 20 %

@Temperature 23.0 °C,
Time 79200 sec
20 %

@Temperature 73.4 °F,
Time 22.0 hour
ASTM D395
40 %

@Temperature 70.0 °C,
Time 79200 sec
40 %

@Temperature 158 °F,
Time 22.0 hour
ASTM D395
Thermal Properties Metric English Comments
Vicat Softening Point 143 °C
289 °F
ASTM D1525
Processing Properties Metric English Comments
Feed Temperature 190 - 205 °C
374 - 401 °F
Nozzle Temperature 200 - 215 °C
392 - 419 °F
Mold Temperature 10.0 - 40.0 °C
50.0 - 104 °F
Drying Temperature 70.0 - 80.0 °C
158 - 176 °F
Dry Time 4.00 - 5.00 hour
4.00 - 5.00 hour
Injection Pressure 11.7 - 15.9 MPa
1700 - 2300 psi
Hold Pressure 8.27 - 12.4 MPa
1200 - 1800 psi
Back Pressure 0.207 - 0.552 MPa
30.0 - 80.0 psi
Cycle Time - Injection 25 - 35 sec
25 - 35 sec
Screw Speed 180 - 220 rpm
180 - 220 rpm
Descriptive Properties Value Comments
Injection time (s) 12-18
Metering Zone 200-215°C