Material Notes:
TLS Chipper Knife tool steel is an air-hardening, 8% chromium tool steel which exhibits very good wear resistance and toughness. TLS Chipper Knife exhibits wear resistance which is better than that of S7, and toughness which is better than that of D2. Typical applications include wood chipper knives, slitter knives, scrap shears, plastic granulator knives, tire shredding knives, shear blades, planer knives, punches, and fineblanking dies.Information Provided by Timken Latrobe Steel.Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.
Physical Properties Metric English Comments
Specific Gravity 7.75 g/cc
7.75 g/cc
Density 7.72 g/cc
0.279 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell C 59
59
Air Cooled from 1010°C, 30 minutes
60
60
Air Cooled from 1038°C, 30 minutes
61
61
Air Cooled from 1052°C, 20 minutes
Modulus of Elasticity 200 GPa
29000 ksi
Machinability 70 - 75 %
70 - 75 %
1% Carbon Steel
Thermal Properties Metric English Comments
CTE, linear 11.3 µm/m-°C

@Temperature 20.0 - 400 °C
6.28 µin/in-°F

@Temperature 68.0 - 752 °F
11.6 µm/m-°C

@Temperature 20.0 - 200 °C
6.44 µin/in-°F

@Temperature 68.0 - 392 °F
Thermal Conductivity 26.1 W/m-K

@Temperature 20.0 °C
181 BTU-in/hr-ft²-°F

@Temperature 68.0 °F
27.1 W/m-K

@Temperature 200 °C
188 BTU-in/hr-ft²-°F

@Temperature 392 °F
28.6 W/m-K

@Temperature 400 °C
198 BTU-in/hr-ft²-°F

@Temperature 752 °F
Component Elements Properties Metric English Comments
Carbon, C 0.50 %
0.50 %
Chromium, Cr 8.0 %
8.0 %
Iron, Fe 88.35 %
88.35 %
Manganese, Mn 0.45 %
0.45 %
Molybdenum, Mo 1.3 %
1.3 %
Silicon, Si 0.95 %
0.95 %
Vanadium, V 0.45 %
0.45 %