Latrobe LSSâ„¢ 2714T Hot Work Tool Steel (DIN 1.2714 mod)

Category Metal , Ferrous Metal , Alloy Steel , Tool Steel , Hot Work Steel
Manufacturer Latrobe Steel
Trade Name LSS™
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Latrobe LSSâ„¢ 2714T Hot Work Tool Steel (DIN 1.2714 mod).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
TLS 2714HT is the same steel available from inventory in a heat-treated condition, at a hardness of 352 to 401 HBS (approximately 38 to 43 HRC). TLS 2714HT can be readily flame cut, and this property is often used to advantage in manufacturing hot extrusion die backer plates. TLS 2714HT should be considered for applications which require higher tensile strengths than the common pre-hardened steels such as 4140 and 4340.Information Provided by Timken Latrobe Steel.Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.
Mechanical Properties Metric English Comments
Hardness, Rockwell C 53
53
Air Cooled from 860°C, 45 minutes
55
55
Oil Quenched from 830°C, 45 minutes
57
57
Air Cooled from 900°C, 45 minutes
59
59
Oil Quenched from 870°C, 45 minutes
Machinability 75 - 80 %
75 - 80 %
1% Carbon Steel
Thermal Properties Metric English Comments
CTE, linear 12.2 µm/m-°C

@Temperature 20.0 - 100 °C
6.78 µin/in-°F

@Temperature 68.0 - 212 °F
14.2 µm/m-°C

@Temperature 20.0 - 500 °C
7.89 µin/in-°F

@Temperature 68.0 - 932 °F
Thermal Conductivity 35.0 W/m-K

@Temperature 700 °C
243 BTU-in/hr-ft²-°F

@Temperature 1290 °F
36.0 W/m-K

@Temperature 20.0 °C
250 BTU-in/hr-ft²-°F

@Temperature 68.0 °F
38.0 W/m-K

@Temperature 350 °C
264 BTU-in/hr-ft²-°F

@Temperature 662 °F
Component Elements Properties Metric English Comments
Carbon, C 0.50 %
0.50 %
Chromium, Cr 1.3 %
1.3 %
Iron, Fe 94.85 %
94.85 %
Manganese, Mn 0.85 %
0.85 %
Molybdenum, Mo 0.50 %
0.50 %
Nickel, Ni 1.65 %
1.65 %
Silicon, Si 0.25 %
0.25 %
Vanadium, V 0.10 %
0.10 %
Chemical Properties Metric English Comments
Critical Temperature 732 °C
1350 °F
Ac1
771 °C
1420 °F
Ac3