Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Ipiranga Petrochem MB 0435 MDPE

Category Polymer , Film , Thermoplastic , Polyethylene (PE) , MDPE , Medium Density Polyethylene (MDPE), Film Grade
Manufacturer Ipiranga Petrochem
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Ipiranga Petrochem MB 0435 MDPE.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
IPQ employs Spherilene technology from Basell in the production of MDPE. The raw materials, which are supplied by COPESUL, are pre-treated and fed into gas-phase reactors, where medium density polyethylene globe-shaped grains are obtained. These grains are sent to the extrusion site, where stabilizers are added to them. The grains are turned into pellets by an extruding press. Next, they are sent to storage silos, and then to the packaging site. This technology uses state-of-the-art techniques to control the entire production process, thus ensuring the quality of the products that are marketed.Applications:back sheet for diapershygienic articles
Physical Properties Metric English Comments
Density 0.933 g/cc
0.0337 lb/in³
ASTM D1505-98
Melt Flow 3.2 - 4.8 g/10 min

@Load 2.16 kg,
Temperature 190 °C
3.2 - 4.8 g/10 min

@Load 4.76 lb,
Temperature 374 °F
ASTM D1238-00
Mechanical Properties Metric English Comments
Tensile Strength at Break 39.0 MPa
5660 psi
ASTM D638-03
Tensile Strength, Yield 20.0 MPa
2900 psi
ASTM D638-02
Elongation at Break 880 %
880 %
ASTM D638-02
Elongation at Yield 12 %
12 %
ASTM D638-02
Flexural Modulus 0.590 GPa
85.6 ksi
2% secant; ASTM D790-02
Izod Impact, Notched 1.15 J/cm
2.15 ft-lb/in
ASTM D256-03
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 61.0 °C
142 °F
ASTM D648-97
Vicat Softening Point 116 °C
241 °F
ASTM D1525-97
Users viewing this material also viewed the following: