Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Industrial Laminates/Norplex NP193P Synthetic Fabric

Category Polymer , Thermoset , Aramid , Phenolic
Manufacturer Industrial Laminates/Norplex
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Industrial Laminates/Norplex NP193P Synthetic Fabric.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Description: 17 oz. aramid and "soft glass" fibers are combined to make a fabric that is stronger than pure aramid and less abrasive than glass fabrics. This material is impregnated with a high temperature phenolic resin matrix, which produces a composite with excellent mechanical strength at elevated temperatures and adverse environments. Applications include wear plates for conveyor systems, valve plates, and compressor and pump vanes. Variations of this material may be developed for specific applications.Thickness Tested: 0.125", 0.250" & 0.500"
Physical Properties Metric English Comments
Moisture Absorption at Equilibrium 3.69 %

@Thickness 1.57 mm
3.69 %

@Thickness 0.0620 in
ASTM D229
Mechanical Properties Metric English Comments
Tensile Strength, Yield 131 MPa

@Thickness 1.57 mm
19000 psi

@Thickness 0.0620 in
CW; ASTM D638
159 MPa

@Thickness 1.57 mm
23000 psi

@Thickness 0.0620 in
LW; ASTM D638
Modulus of Elasticity 8.27 GPa

@Thickness 1.57 mm
1200 ksi

@Thickness 0.0620 in
CW; ASTM D229
8.27 GPa

@Thickness 1.57 mm
1200 ksi

@Thickness 0.0620 in
LW; ASTM D229
Flexural Strength 103 MPa

@Thickness 1.57 mm
15000 psi

@Thickness 0.0620 in
CW; ASTM D790
228 MPa

@Thickness 1.57 mm
33000 psi

@Thickness 0.0620 in
LW; ASTM D790
Compressive Strength 269 MPa

@Thickness 12.7 mm
39000 psi

@Thickness 0.500 in
ASTM D695
Izod Impact, Unnotched 3.74 J/cm

@Thickness 12.7 mm
7.00 ft-lb/in

@Thickness 0.500 in
CW, Cond E-48/50; ASTM D256
12.8 J/cm

@Thickness 12.7 mm
24.0 ft-lb/in

@Thickness 0.500 in
LW, Cond E-48/50; ASTM D256
Thermal Properties Metric English Comments
CTE, linear 21.0 µm/m-°C

@Thickness 1.57 mm,
Temperature 20.0 °C
11.7 µin/in-°F

@Thickness 0.0620 in,
Temperature 68.0 °F
x-axis; IPC-TM 650-2.4.24
CTE, linear, Transverse to Flow 30.8 µm/m-°C

@Thickness 1.57 mm,
Temperature 20.0 °C
17.1 µin/in-°F

@Thickness 0.0620 in,
Temperature 68.0 °F
x-axis; IPC-TM 650-2.4.24
Flammability, UL94 HB

@Thickness 1.57 mm
HB

@Thickness 0.0620 in
Electrical Properties Metric English Comments
Dielectric Constant 5.0

@Thickness 1.57 mm
5.0

@Thickness 0.0620 in
Permittivity, Cond D-24/23; ASTM D150
Dissipation Factor 0.030

@Thickness 1.57 mm
0.030

@Thickness 0.0620 in
Cond D-24/23; ASTM D150
Descriptive Properties Value Comments
Bond Strength 2400 lb
0.5", ASTM D229
Color Natural