Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Hexcel® HexPly® F522 Epoxy Resin, K285 Kevlar® Fabric

Category Polymer , Thermoset , Epoxy , Epoxy Cure Resin
Manufacturer Hexcel
Trade Name HexPly®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Hexcel® HexPly® F522 Epoxy Resin, K285 Kevlar® Fabric.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Hexcel designation: K285-38"-F522; Kev. 49 1140Information provided by HexCel
Mechanical Properties Metric English Comments
Tensile Strength, Yield 517 MPa

@Temperature 24.0 °C
75000 psi

@Temperature 75.2 °F
Dry
Tensile Modulus 29.0 GPa

@Temperature 24.0 °C
4210 ksi

@Temperature 75.2 °F
Dry
Flexural Yield Strength 110 MPa

@Temperature 24.0 °C
16000 psi

@Temperature 75.2 °F
Long Beam, Dry
414 MPa

@Temperature 24.0 °C
60000 psi

@Temperature 75.2 °F
Dry
Compressive Yield Strength 117 MPa

@Temperature 71.0 °C
17000 psi

@Temperature 160 °F
Wet (14 ± 1/2 days of water immersion at 160 ± 5°F (71 ± 3°C)
179 MPa

@Temperature 24.0 °C
26000 psi

@Temperature 75.2 °F
Dry
Compressive Modulus 25.5 GPa

@Temperature 71.0 °C
3700 ksi

@Temperature 160 °F
Wet (14 ± 1/2 days of water immersion at 160 ± 5°F (71 ± 3°C)
30.3 GPa

@Temperature 24.0 °C
4390 ksi

@Temperature 75.2 °F
Dry
Descriptive Properties Value Comments
Dry Resin Content (%) 49-55
Prepreg
Fiber Volume (%) 0.025
Laminate
Flow (%) 20-32
Wet Resin Content (%) 46
Laminate