Material Notes:
A thermoset polyester composite that offers superior energy efficiency, temperature control, and durability for high temperature mold and platen thermal applications. A proven, cost effective product for the plastic and rubber molder. Available in thicknesses from 1/8" - 2.00". Color - Brown.Information provided by Haysite
Physical Properties Metric English Comments
Water Absorption 0.25 %

@Thickness 9.52 mm
0.25 %

@Thickness 0.375 in
ASTM D570
Mechanical Properties Metric English Comments
Tensile Strength 82.7 MPa
12000 psi
ASTM D638
Tensile Modulus 11.0 GPa
1600 ksi
ASTM D638
Flexural Strength 159 MPa
23000 psi
ASTM D790
Compressive Strength 290 MPa
42000 psi
ASTM D695
111 MPa

@Temperature 204 °C
16100 psi

@Temperature 400 °F
ASTM D695
161 MPa

@Temperature 149 °C
23400 psi

@Temperature 300 °F
ASTM D695
Poissons Ratio 0.332
0.332
ASTM E132
Shear Modulus 4.13 GPa
599 ksi
Calculated
Izod Impact, Notched 5.34 J/cm
10.0 ft-lb/in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear 14.0 µm/m-°C
7.78 µin/in-°F
ASTM D696
Thermal Conductivity 1.90 W/m-K
13.2 BTU-in/hr-ft²-°F
ASTM D177
Maximum Service Temperature, Inert 232 °C
450 °F