ExxonMobil LLDPE LL 1002YB Cast Linear Low Density Polyethylene Resin

Category Polymer , Thermoplastic , Polyethylene (PE) , LLDPE
Manufacturer Exxon Chemical
Trade Name LLDPE
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF ExxonMobil LLDPE LL 1002YB Cast Linear Low Density Polyethylene Resin.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Product Description: LL 1002YB is an LLDPE resin designed for cast films. It offers high gloss and excellent drawdown in both blown and cast film applications. LL 1002YB may also be used as a blend partner with LDPE resins to improve film properties and processability. Availability: Africa & Middle East, Asia Pacific, Europe, Latin America, North America and South America Additive: Antiblock: NoSlip: No Processing Aid: NoThermal Stabilizer: YesApplications: Cast FilmCast Stretch FilmGarment FilmGeneral PackagingHygiene filmPackaging FilmsPersonal CareInformation provided by ExxonMobil
Physical Properties Metric English Comments
Density 0.918 g/cc
0.0332 lb/in³
ExxonMobil method
Melt Flow 2.0 g/10 min

@Load 2.16 kg,
Temperature 190 °C
2.0 g/10 min

@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Mechanical Properties Metric English Comments
Film Tensile Strength at Yield, MD 7.58 MPa
1100 psi
ASTM D882
Film Tensile Strength at Yield, TD 6.48 MPa
940 psi
ASTM D882
Film Elongation at Break, MD 420 %
420 %
ASTM D882
Film Elongation at Break, TD 830 %
830 %
ASTM D882
Puncture Energy 2.37 J
1.75 ft-lb
ExxonMobil Method
Elmendorf Tear Strength MD 20 g
20 g
ASTM D1922
Elmendorf Tear Strength TD 430 g
430 g
ASTM D1922
Dart Drop Test <= 50.0 g
<= 0.110 lb
ASTM D1709A
Film Tensile Strength at Break, MD 62.1 MPa
9000 psi
ASTM D882
Film Tensile Strength at Break, TD 24.8 MPa
3600 psi
ASTM D882
1% Secant Modulus, MD 117 MPa
17000 psi
ASTM D882
1% Secant Modulus, TD 131 MPa
19000 psi
ASTM D882
Thermal Properties Metric English Comments
Melting Point <= 248 °C
<= 478 °F
Peak Melting Point; ExxonMobil method
Optical Properties Metric English Comments
Haze 1.7 %
1.7 %
ASTM D1003
Gloss 98 %
98 %
45°; ASTM D2457
Descriptive Properties Value Comments
Puncture Force 8 lbf
ExxonMobil Method
Copyright © lookpolymers.com All Rights Reserved