Material Notes:
Vamac® DP is an ethylene acrylic dipolymer elastomer. Its general performance characteristics are similar to those of the Vamac® terpolymers, including:Good oil and chemical resistanceHigh temperature resistanceGood compression set resistanceGood low temperature flexibilityUnlike Vamac® terpolymers, Vamac® DP dipolymer can be processed without a post cure.Form: Bale size is nominally:560 mm x 370 mm by 165 mmInformation provided by DuPont.
Physical Properties Metric English Comments
Mooney Viscosity 43.6

@Temperature 100 °C
43.6

@Temperature 212 °F
ML(1+4), mu; ASTM D1646
Mechanical Properties Metric English Comments
Hardness, Shore A 64
64
No Scale (Assumed Shore A); ASTM D2240
Tensile Strength, Ultimate 18.2 MPa
2640 psi
ASTM D412
Elongation at Break 208 %
208 %
ASTM D412
100% Modulus 0.00720 GPa
1.04 ksi
ASTM D412
Compression Set 21.5 %
21.5 %
72 hrs at 150°C; ASTM D395
23 %
23 %
168 hrs at 150°C; ASTM D395
43.4 %
43.4 %
1008 hrs at 150°C; ASTM D395
Descriptive Properties Value Comments
Armeen® 18D 0.5 phr
HVA® #2 coagent 2 phr
Mooney Scorch at 135°C, Minimum Viscosity 11.6
Mooney units
Mooney Scorch at 135°C, t10 11.3 minutes
Time for 10 unit rise
Mooney Scorch at 135°C, t3 8.2 minutes
Time for 3 unit rise
N550 Black 55 phr
Naugard® 445 antioxidant 1 phr
Stearic Acid 0.5 phr
Vamac® DP 100 phr
Vanfre® VAM 1.25 phr
Vulcup® 40LE peroxide 5.5 phr