Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

DSM Stanyl® TW441 Nylon 46 (European and Asian Grade) (Dry)

Category Polymer , Thermoplastic , Nylon , Nylon 46 , Nylon 46, Unreinforced
Manufacturer DSM Engineering Plastics
Trade Name Stanyl®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF DSM Stanyl® TW441 Nylon 46 (European and Asian Grade) (Dry).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Stanyl is a high performance polyamide providing unmatched performance and value across an amazingly broad range of automotive and electronic applications. Stanyl offers:Highest mechanical properties at high temperatures Excellent resistance to wear and low friction Outstanding flow for easy processing and exceptional design freedomStanyl High Flowgrades that match the best flowing LCPs while maintaining a high level of mechanical propertiesKey Applications: Automotive: Powertrain components, Charge-air coolers, EPS and ETC gears, Motor Sensors, Auto connectors, Chain tensionersE&E: Connectors, Microswitches, Bobbins, Memory modules, Motor components, Industrial, Specialty films and fibers, Consumer appliancesInformation provided by DSM.
Physical Properties Metric English Comments
Density 1.18 g/cc
0.0426 lb/in³
ISO 1183
Viscosity Test 220 cm³/g
220 cm³/g
Viscosity Number
Linear Mold Shrinkage, Flow 0.020 cm/cm
0.020 in/in
ISO 294-4
Linear Mold Shrinkage, Transverse 0.020 cm/cm
0.020 in/in
ISO 294-4
Mechanical Properties Metric English Comments
Tensile Strength, Yield 100 MPa
14500 psi
ISO 527-1/-2
Elongation at Break 40 %
40 %
ISO 527-1/-2
Elongation at Yield 10 %
10 %
ISO 527-1/-2
Tensile Modulus 3.30 GPa
479 ksi
ISO 527-1/-2
Charpy Impact Unnotched NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
ISO 179/1eU
NB

@Temperature 23.0 °C
NB

@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.900 J/cm²

@Temperature -30.0 °C
4.28 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eA
1.20 J/cm²

@Temperature 23.0 °C
5.71 ft-lb/in²

@Temperature 73.4 °F
ISO 179/1eA
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 80.0 µm/m-°C

@Temperature 20.0 °C
44.4 µin/in-°F

@Temperature 68.0 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°C

@Temperature 20.0 °C
55.6 µin/in-°F

@Temperature 68.0 °F
ISO 11359-1/-2
Melting Point 295 °C
563 °F
10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 280 °C
536 °F
ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 190 °C
374 °F
ISO 75-1/-2
Vicat Softening Point 290 °C
554 °F
50°C/h 50N; ISO 306
Glass Transition Temp, Tg 75.0 °C
167 °F
Glass Transition Temperature (10°C/min); ISO 11357-1/-2
Flammability, UL94 V-2

@Thickness 0.750 mm
V-2

@Thickness 0.0295 in
IEC 60695-11-10
V-2

@Thickness 1.60 mm
V-2

@Thickness 0.0630 in
IEC 60695-11-10
Descriptive Properties Value Comments
Injection molding Yes
Other Extrusion Yes
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved