Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Crucible Steel WR-95 Tool Steel, AISI H10 Modified

Category Metal , Ferrous Metal , Tool Steel
Manufacturer Crucible Steel
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Crucible Steel WR-95 Tool Steel, AISI H10 Modified.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
WR-95 is a modified H10, with cobalt added to improve its high temperature properties. It is an upgrade from H13 in applications requiring improved hot hardness or heat check resistance, at a slight decrease in toughness. It may be used at tool temperatures up to about 1100F, with brief exposures up to about 1200F.Information provided by Crucible Industries
Physical Properties Metric English Comments
Density 7.83 g/cc
0.283 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell C 40.5

@Tempering Temp. 649 °C
40.5

@Tempering Temp. 1200 °F
air cooled from 1900°F then tempered
50.5

@Tempering Temp. 621 °C
50.5

@Tempering Temp. 1150 °F
air cooled from 1900°F then tempered
54.5

@Tempering Temp. 593 °C
54.5

@Tempering Temp. 1100 °F
air cooled from 1900°F then tempered
57

@Tempering Temp. 566 °C
57

@Tempering Temp. 1050 °F
air cooled from 1900°F then tempered
58

@Tempering Temp. 538 °C
58

@Tempering Temp. 1000 °F
air cooled from 1900°F then tempered
Modulus of Elasticity 207 GPa
30000 ksi
Charpy Impact 12.2 J

@Tempering Temp. 538 °C
9.00 ft-lb

@Tempering Temp. 1000 °F
air cooled from 1900°F then tempered; V-notch
13.6 J

@Tempering Temp. 566 °C
10.0 ft-lb

@Tempering Temp. 1050 °F
air cooled from 1900°F then tempered; V-notch
16.3 J

@Tempering Temp. 593 °C
12.0 ft-lb

@Tempering Temp. 1100 °F
air cooled from 1900°F then tempered; V-notch
19.0 J

@Tempering Temp. 621 °C
14.0 ft-lb

@Tempering Temp. 1150 °F
air cooled from 1900°F then tempered; V-notch
21.0 J

@Tempering Temp. 649 °C
15.5 ft-lb

@Tempering Temp. 1200 °F
air cooled from 1900°F then tempered; V-notch
Thermal Properties Metric English Comments
CTE, linear 11.3 µm/m-°C

@Temperature 21.1 - 93.3 °C
6.30 µin/in-°F

@Temperature 70.0 - 200 °F
11.7 µm/m-°C

@Temperature 21.1 - 260 °C
6.50 µin/in-°F

@Temperature 70.0 - 500 °F
12.1 µm/m-°C

@Temperature 21.1 - 427 °C
6.70 µin/in-°F

@Temperature 70.0 - 800 °F
12.8 µm/m-°C

@Temperature 21.1 - 538 °C
7.10 µin/in-°F

@Temperature 70.0 - 1000 °F
13.3 µm/m-°C

@Temperature 21.1 - 649 °C
7.40 µin/in-°F

@Temperature 70.0 - 1200 °F
Thermal Conductivity 2.16 W/m-K

@Temperature 93.3 °C
15.0 BTU-in/hr-ft²-°F

@Temperature 200 °F
Component Elements Properties Metric English Comments
Carbon, C 0.35 %
0.35 %
Chromium, Cr 3.5 %
3.5 %
Cobalt, Co 2.0 %
2.0 %
Iron, Fe 89.85 %
89.85 %
as balance
Manganese, Mn 0.30 %
0.30 %
Molybdenum, Mo 2.5 %
2.5 %
Silicon, Si 0.90 %
0.90 %
Vanadium, V 0.60 %
0.60 %
Chemical Properties Metric English Comments
Critical Temperature 843 °C
1550 °F
Users viewing this material also viewed the following: