Material Notes:
Gorilla® Glass 3 with Native Damage Resistance™ (NDR) is an alkali-aluminosilicate thin sheet glass that is better able to survive the real-world events that most commonly cause glass failure. With its core composition, this glass enables improved damage resistance and toughness by helping to prevent the deep chips and scratches that cause glass to break. This glass is widely used in smart phone, tablet, and laptop displays, other touchscreens, optical components, and other high strength glass applications.Information provided by Corning Incorporated.
Physical Properties Metric English Comments
Density 2.39 g/cc
0.0863 lb/in³
Thickness 400 - 2000 microns
15.7 - 78.7 mil
Mechanical Properties Metric English Comments
Vickers Microhardness 534
534
kgf/mm²; unstrengthened (200 g load)
649
649
kgf/mm²; strengthened (200 g load)
Modulus of Elasticity 69.3 GPa
10100 ksi
Compressive Strength 950 MPa
138000 psi
Chemically Strengthened to 40 µm Depth
Poissons Ratio 0.22
0.22
Fracture Toughness 0.660 MPa-m½
0.601 ksi-in½
Shear Modulus 28.5 GPa
4130 ksi
Thermal Properties Metric English Comments
CTE, linear 7.58 µm/m-°C

@Temperature 0.000 - 300 °C
4.21 µin/in-°F

@Temperature 32.0 - 572 °F
Softening Point 900 °C
1650 °F
10<sup>7.6</sup> Poise
Annealing Point 628 °C
1160 °F
10<sup>13.2</sup> Poise
Strain Point 574 °C
1070 °F
10<sup>14.7</sup> Poise
Optical Properties Metric English Comments
Refractive Index 1.50

@Wavelength 590 nm
1.50

@Wavelength 590 nm
core glass
1.51

@Wavelength 590 nm
1.51

@Wavelength 590 nm
compression layer
Transmission, Visible >= 91.5 %

@Wavelength 390 - 800 nm
>= 91.5 %

@Wavelength 390 - 800 nm
IR Transmittance >= 90.0 %

@Wavelength 2200 - 2500 nm
>= 90.0 %

@Wavelength 2200 - 2500 nm
>= 91.5 %

@Wavelength 700 - 2200 nm
>= 91.5 %

@Wavelength 700 - 2200 nm
UV Transmittance 0.0 %

@Wavelength <=250 nm
0.0 %

@Wavelength <=250 nm
Electrical Properties Metric English Comments
Dielectric Constant 7.19

@Frequency 2.986e+9 Hz
7.19

@Frequency 2.986e+9 Hz
7.20

@Frequency 2.466e+9 Hz
7.20

@Frequency 2.466e+9 Hz
7.23

@Frequency 1.977e+9 Hz
7.23

@Frequency 1.977e+9 Hz
7.26

@Frequency 1.50e+9 Hz
7.26

@Frequency 1.50e+9 Hz
7.30

@Frequency 9.1e+8 Hz
7.30

@Frequency 9.1e+8 Hz
7.37

@Frequency 5.990e+8 Hz
7.37

@Frequency 5.990e+8 Hz
7.38

@Frequency 4.90e+8 Hz
7.38

@Frequency 4.90e+8 Hz
7.42

@Frequency 3.81e+8 Hz
7.42

@Frequency 3.81e+8 Hz
7.44

@Frequency 2.72e+8 Hz
7.44

@Frequency 2.72e+8 Hz
7.48

@Frequency 1.63e+8 Hz
7.48

@Frequency 1.63e+8 Hz
7.59

@Frequency 5.40e+7 Hz
7.59

@Frequency 5.40e+7 Hz
Dissipation Factor 0.0210

@Frequency 4.90e+8 Hz
0.0210

@Frequency 4.90e+8 Hz
0.0210

@Frequency 2.72e+8 Hz
0.0210

@Frequency 2.72e+8 Hz
0.0220

@Frequency 3.81e+8 Hz
0.0220

@Frequency 3.81e+8 Hz
0.0220

@Frequency 5.4e+7 Hz
0.0220

@Frequency 5.4e+7 Hz
0.0220

@Frequency 1.63e+8 Hz
0.0220

@Frequency 1.63e+8 Hz
0.0230

@Frequency 5.99e+8 Hz
0.0230

@Frequency 5.99e+8 Hz
0.0230

@Frequency 9.12e+8 Hz
0.0230

@Frequency 9.12e+8 Hz
0.0230

@Frequency 1.499e+9 Hz
0.0230

@Frequency 1.499e+9 Hz
0.0230

@Frequency 1.977e+9 Hz
0.0230

@Frequency 1.977e+9 Hz
0.0240

@Frequency 2.466e+9 Hz
0.0240

@Frequency 2.466e+9 Hz
0.0250

@Frequency 2.986e+9 Hz
0.0250

@Frequency 2.986e+9 Hz
Descriptive Properties Value Comments
Photo-elastic Constant 31.9 nm/cm/MPa