Celanese Celstran® TPU-GF60-01-US TPU, 60% Glass Reinforced

Category Polymer , Thermoplastic , Polyurethane, TP , Thermoplastic Polyurethane (TPUR), Glass Fiber Reinforced
Manufacturer Celanese Corporation
Trade Name CELSTRAN
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Celanese Celstran® TPU-GF60-01-US TPU, 60% Glass Reinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
60% long strand glass fiber reinforced thermoplastic polyurethaneInformation provided by Celanese
Physical Properties Metric English Comments
Specific Gravity 1.76 g/cc
1.76 g/cc
ASTM D792
Density 1.76 g/cc
0.0636 lb/in³
ISO 1183
Linear Mold Shrinkage, Flow 0.000500 - 0.00100 cm/cm
0.000500 - 0.00100 in/in
ASTM D955
Linear Mold Shrinkage, Transverse 0.000500 - 0.00100 cm/cm
0.000500 - 0.00100 in/in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 240 MPa
34800 psi
5mm/min; ISO 527-2/1A
259 MPa
37500 psi
ASTM D638
Elongation at Break 1.70 %
1.70 %
ASTM D638
1.75 %
1.75 %
5mm/min; ISO 527-2/1A
Tensile Modulus 18.7 GPa
2710 ksi
50mm/min; ISO 527-2/1A
19.9 GPa
2880 ksi
ASTM D638
Flexural Strength 407 MPa
59100 psi
ASTM D790
420 MPa
60900 psi
ISO 178
Flexural Modulus 16.4 GPa
2380 ksi
ASTM D790
18.3 GPa
2650 ksi
ISO 178
Izod Impact, Notched 8.44 J/cm
15.8 ft-lb/in
ASTM D256
Charpy Impact, Notched 6.60 J/cm²
31.4 ft-lb/in²
ISO 179/1eA
Thermal Properties Metric English Comments
Deflection Temperature at 1.8 MPa (264 psi) 102 °C
215 °F
ASTM D648
102 °C
216 °F
ISO 75-1, -2
Processing Properties Metric English Comments
Processing Temperature 70.0 - 90.0 °C
158 - 194 °F
cavity
250 - 265 °C
482 - 509 °F
hot runner
Feed Temperature 20.0 - 50.0 °C
68.0 - 122 °F
Middle Barrel Temperature 70.0 - 80.0 °C
158 - 176 °F
Zone 1 240 - 250 °C
464 - 482 °F
Zone 2 245 - 255 °C
473 - 491 °F
Zone 3 245 - 260 °C
473 - 500 °F
Zone 4 245 - 260 °C
473 - 500 °F
Die Temperature 245 - 260 °C
473 - 500 °F
Melt Temperature 245 - 260 °C
473 - 500 °F
Drying Temperature 80.0 °C
176 °F
Dry Time 4.00 hour
4.00 hour
Moisture Content <= 0.0500 %
<= 0.0500 %
Descriptive Properties Value Comments