Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Celanese Celanex® 2300 GV1/10 PBT, 10% Glass Reinforced  (Unverified Data**)

Category Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) , Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled
Manufacturer
Trade Name Celanex®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Celanese Celanex® 2300 GV1/10 PBT, 10% Glass Reinforced  (Unverified Data**).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Chemical abbreviation according to ISO 1043-1: PBTGeneral purpose, 10% glass fiber reinforced PBTInformation provided by Celanese
Physical Properties Metric English Comments
Density 1.38 g/cc
0.0499 lb/in³
ISO 1183
Density of Compound 1.17 g/cc
0.0423 lb/in³
melt; Internal
Moisture Absorption 0.200 %
0.200 %
23°C/50%RH; ISO 62
Viscosity Test 80 cm³/g
80 cm³/g
ISO 307, 1157, 1628
Melt Flow 21 g/10 min

@Load 2.16 kg,
Temperature 250 °C
21 g/10 min

@Load 4.76 lb,
Temperature 482 °F
(MVR) cm³/10min; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 90.0 MPa
13100 psi
5mm/min; ISO 527-2/1A
Elongation at Break 3.5 %
3.5 %
5mm/min; ISO 527-2/1A
Tensile Modulus 4.70 GPa
682 ksi
1mm/min; ISO 527-2/1A
Flexural Strength 130 MPa
18900 psi
ISO 178
Charpy Impact Unnotched 2.60 J/cm²
12.4 ft-lb/in²
ISO 179/1eU
2.60 J/cm²

@Temperature -30.0 °C
12.4 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.500 J/cm²
2.38 ft-lb/in²
ISO 179/1eA
0.500 J/cm²

@Temperature -30.0 °C
2.38 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eA
Tensile Creep Modulus, 1 hour 4600 MPa
667000 psi
ISO 899-1
Tensile Creep Modulus, 1000 hours 3500 MPa
508000 psi
ISO 899-1
Thermal Properties Metric English Comments
CTE, linear 60.0 µm/m-°C
33.3 µin/in-°F
ISO 11359-2
Specific Heat Capacity 1.87 J/g-°C
0.447 BTU/lb-°F
Internal
Thermal Conductivity 0.144 W/m-K
0.999 BTU-in/hr-ft²-°F
Internal
Melting Point 225 °C
437 °F
10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 210 °C
410 °F
ISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 190 °C
374 °F
ISO 75-1, -2
Deflection Temperature at 8.0 MPa 60.0 °C
140 °F
ISO 75-1, -2
Vicat Softening Point 205 °C
401 °F
B50 (50°C/h 50N); ISO 306
Flammability, UL94 HB

@Thickness 1.60 mm
HB

@Thickness 0.0630 in
UL94
HB

@Thickness 1.22 mm
HB

@Thickness 0.0480 in
UL94
Oxygen Index 19 %
19 %
ISO 4589
Electrical Properties Metric English Comments
Volume Resistivity >= 1.00e+15 ohm-cm
>= 1.00e+15 ohm-cm
IEC 60093
Surface Resistance >= 1.00e+15 ohm
>= 1.00e+15 ohm
IEC 60093
Dielectric Constant 3.9

@Frequency 1.00e+6 Hz
3.9

@Frequency 1.00e+6 Hz
IEC 60250
4.0

@Frequency 100 Hz
4.0

@Frequency 100 Hz
IEC 60250
Dielectric Strength 28.0 kV/mm
711 kV/in
IEC 60243-1
Dissipation Factor 0.0013

@Frequency 100 Hz
0.0013

@Frequency 100 Hz
IEC 60250
0.019

@Frequency 1.00e+6 Hz
0.019

@Frequency 1.00e+6 Hz
IEC 60250
Comparative Tracking Index 325 V
325 V
IEC 60112
Processing Properties Metric English Comments
Processing Temperature 20.0 - 50.0 °C
68.0 - 122 °F
75.0 - 100 °C
167 - 212 °F
Cavity temperature
219 °C
426 °F
Ejection temperature; Internal
Feed Temperature 190 - 200 °C
374 - 392 °F
Zone 1 250 - 260 °C
482 - 500 °F
Zone 2 250 - 260 °C
482 - 500 °F
Zone 3 255 - 265 °C
491 - 509 °F
Zone 4 255 - 265 °C
491 - 509 °F
Die Temperature 260 - 270 °C
500 - 518 °F
Melt Temperature 260 - 270 °C
500 - 518 °F
265 °C
509 °F
Injection molding; ISO 294
Mold Temperature 75.0 - 85.0 °C
167 - 185 °F
80.0 °C
176 °F
Injection molding; ISO 294
Injection Velocity 200 mm/sec
7.87 in/sec
ISO 294
Drying Temperature 120 - 140 °C
248 - 284 °F
Dry Time 2.00 - 4.00 hour
2.00 - 4.00 hour
Moisture Content 0.020 %
0.020 %
Necessary low maximum residual
Dew Point <= -30.0 °C
<= -22.0 °F
Pre-drying
Hold Pressure 40.0 - 80.0 MPa
5800 - 11600 psi
70.0 MPa
10200 psi
ISO 294
60.0 - 100 MPa
8700 - 14500 psi
Back Pressure 1.00 - 3.00 MPa
145 - 435 psi
Screw Speed 60 rpm

@Diameter 55.0 mm
60 rpm

@Diameter 2.17 in
75 rpm

@Diameter 40.0 mm
75 rpm

@Diameter 1.57 in
90 rpm

@Diameter 25.0 mm
90 rpm

@Diameter 0.984 in
Hot-Working Temperature 260 - 270 °C
500 - 518 °F
Descriptive Properties Value Comments
Injection molding Yes
Injection Speed fast
Longer pre-drying times/storage lower the temperature to 100° C until processed.
<= 60 h
Processing conditions 7792
Processing Notes Fast Injection Speed
Maximum Barrel Residence Time 5-10  min
Open Nozzle Design Preferred
Peripheral screw speed max. 0.3  m/sec
Copyright © lookpolymers.com All Rights Reserved