Material Notes:
Data provided by Carpenter Technology Corporation.This is a carburizing steel possessing good temper resistance and high case hot hardness while maintaining high core impact strength and fracture toughness. This alloy has been used in gears where temperature resistance is important.Pyrowear® is a registered trademark of Carpenter Technology Corporation.
Physical Properties Metric English Comments
Density 7.80 g/cc
0.282 lb/in³
Estimated by MatWeb
Mechanical Properties Metric English Comments
Hardness, Brinell 334
334
Estimated from Rockwell C for 3000 kg load, 10 mm ball Brinell measurement.
Hardness, Knoop 363
363
Estimated from Rockwell C
Hardness, Rockwell C 36
36
Hardness, Vickers 349
349
Estimated from Rockwell C
Tensile Strength, Ultimate 1172 MPa
170000 psi
1207 MPa

@Temperature 177 °C
175100 psi

@Temperature 351 °F
1331 MPa

@Temperature -54.0 °C
193000 psi

@Temperature -65.2 °F
Tensile Strength, Yield 965 MPa
140000 psi
Offset not given
896 MPa

@Temperature 177 °C
130000 psi

@Temperature 351 °F
Offset not given
1103 MPa

@Temperature -54.0 °C
160000 psi

@Temperature -65.2 °F
Offset not given
Elongation at Break 16 %
16 %
12 %

@Temperature 177 °C
12 %

@Temperature 351 °F
18 %

@Temperature -54.0 °C
18 %

@Temperature -65.2 °F
Reduction of Area 66.5 %
66.5 %
46 %

@Temperature 177 °C
46 %

@Temperature 351 °F
63 %

@Temperature -54.0 °C
63 %

@Temperature -65.2 °F
Fracture Toughness 130 MPa-m½
118 ksi-in½
K(Q)
Charpy Impact 130 J
95.9 ft-lb
V-notch
55.0 J

@Temperature -54.0 °C
40.6 ft-lb

@Temperature -65.2 °F
V-notch
155 J

@Temperature 177 °C
114 ft-lb

@Temperature 351 °F
V-notch
Thermal Properties Metric English Comments
CTE, linear 11.26 µm/m-°C

@Temperature 24.0 - 93.0 °C
6.256 µin/in-°F

@Temperature 75.2 - 199 °F
12.06 µm/m-°C

@Temperature 24.0 - 260 °C
6.700 µin/in-°F

@Temperature 75.2 - 500 °F
13.05 µm/m-°C

@Temperature 24.0 - 538 °C
7.250 µin/in-°F

@Temperature 75.2 - 1000 °F
Component Elements Properties Metric English Comments
Carbon, C 0.10 %
0.10 %
Chromium, Cr 1.0 %
1.0 %
Copper, Cu 2.0 %
2.0 %
Iron, Fe 89.5 %
89.5 %
as remainder
Manganese, Mn 0.35 %
0.35 %
Molybdenum, Mo 3.25 %
3.25 %
Nickel, Ni 2.0 %
2.0 %
Silicon, Si 1.0 %
1.0 %
Vanadium, V 0.10 %
0.10 %
Copyright © lookpolymers.com All Rights Reserved