Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

BASF Elastollan® C-70AW Polyester Type Polyurethane Elastomer

Category Polymer , Thermoplastic , Elastomer, TPE , Polyurethane, TP , Thermoplastic Polyurethane, Elastomer, Polyester Grade
Manufacturer BASF
Trade Name Elastollan®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF BASF Elastollan® C-70AW Polyester Type Polyurethane Elastomer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Processed by extrusion or injection molding. Elastollan C series of products are polyester-based thermoplastic polyurethanes that exhibit very good hydrolytic stability. They also exhibit excellent oil, fuel and solvent resistance. These products can be injection and blow molded and extruded. As with all TPU products this grade must be dried prior to processing.Property values below are typical values based on test samples cured 20 hours at 100°C before testing. Information provided by BASF Corporation.
Physical Properties Metric English Comments
Density 1.15 g/cc
0.0415 lb/in³
ASTM D792
Mechanical Properties Metric English Comments
Hardness, Shore A 71
71
ASTM D2240
Tensile Strength, Ultimate 30.0 MPa
4350 psi
ASTM D412
Tensile Strength, Yield 3.10 MPa

@Strain 100 %
450 psi

@Strain 100 %
ASTM D-412
5.60 MPa

@Strain 300 %
812 psi

@Strain 300 %
ASTM D-412
Elongation at Break 790 %
790 %
ASTM D412
Tear Strength 65.0 kN/m
371 pli
ASTM D624
Tensile Set 75 %
75 %
at break; ASTM D-412
Users viewing this material also viewed the following: