Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Advanced Polymer Alloys Alcryn® 2160 BK Melt Processable Rubber

Category Polymer , Thermoplastic , Elastomer, TPE
Manufacturer APA - Advanced Polymer Alloys
Trade Name Alcryn®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Advanced Polymer Alloys Alcryn® 2160 BK Melt Processable Rubber.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Alcryn 2100 Series melt-processable rubber (MPR) offer a broader range of bonding to rigid substrates while maintaining all the excellent performance features of traditional Alcryn. The 2100 grades bond to polycarbonate, ABS, polycarbonate/ABS alloys, SAN, ASA, copolyester elastomers and TPUs, as well as both flexible and rigid PVC. Applications:Injection-molded and overmolded partsSoft touch handles and gripsAutomotive interior applicationsSeals and gaskets for automotive insert moldingNoise and vibration deadeningBlow-molded partsTubing and hoseWire and cable jacketsCoated fabrics and sheet goodsWindow and door weatherstrippingInformation provided by Advanced Polymer Alloys
Physical Properties Metric English Comments
Specific Gravity 1.15 g/cc
1.15 g/cc
ASTM D471
Viscosity 265000 cP

@Shear Rate 300 1/s,
Temperature 190 °C
265000 cP

@Shear Rate 300 1/s,
Temperature 374 °F
ASTM D3835
Mechanical Properties Metric English Comments
Hardness, Shore A 55
55
After 7 days at 125°C; ASTM D573
59
59
ASTM D2240
Tensile Strength at Break 11.1 MPa
1610 psi
ASTM D412
13.432 MPa
1948.1 psi
After 7 days at 125°C; ASTM D573
Elongation at Break 620 %
620 %
ASTM D412
638.6 %
638.6 %
After 7 days at 125°C; ASTM D573
100% Modulus 0.00230 GPa
0.333 ksi
ASTM D412
0.0031225 GPa
0.45288 ksi
After 7 days at 125°C; ASTM D573
Graves Tear Strength 55.01 kN/m

@Temperature 24.0 °C
313.8 pli

@Temperature 75.2 °F
Die C; ASTM D624
Compression Set 18 %
18 %
After 22 Hr At 24°C; ASTM D395
86 %
86 %
After 22 Hr at 100°C; ASTM D395
Tensile Set 14 %
14 %
ASTM D412
Thermal Properties Metric English Comments
Brittleness Temperature -68.0 °C
-90.4 °F
ASTM D746
Clash Berg Stiffness Temperature -49.0 °C
-56.2 °F
69 Mpa; ASTM D1043
Processing Properties Metric English Comments
Processing Temperature 177 °C
351 °F
Descriptive Properties Value Comments
Fluid Resistance - Volume Change, % (ASTM D471) 16
After 7 Days in ASTM Ref. Fuel no. B at 75°F (24°C)
-22
After 7 Days in ASTM Oil No. 1 At 212°F (100°C)
4
After 7 Days in IRM 903 Oil No. 3 at 212°F (100°C)
6
After 7 Days in Water at 212°F (100°C)
Users viewing this material also viewed the following: