Material Notes:
QM 107 is a two component, room temperature condensation cure silicone material. The cured rubber is very soft, has excellent mechanical properties and good shelf-life stability. This material is an excellent choice for the molding of intricate patterns, skin molding or for applications which demand a tough rubber. The hardness of QM 118 is the midpoint of the QM100 series and therefore offers excellent physical properties. A variety of catalysts are offered with this material.  Key Features:Low ViscosityExcellent physical propertiesFast demold timeMain Applications: Molds for small statues, large statues and monument restoration Molds for polyester, polyurethane and epoxy resin castings Molds for prototypes Part of the Amber Chemical Group. Data provided by manufacturer.
Physical Properties Metric English Comments
Specific Gravity 0.950 g/cc
0.950 g/cc
Uncatalyzed, QM CAT RED 3
1.00 g/cc
1.00 g/cc
Uncatalyzed, QM CAT PURPLE
1.03 g/cc
1.03 g/cc
Uncatalyzed, QM CAT BLUE
1.24 g/cc
1.24 g/cc
catalyzed with QM CAT PURPLE
1.24 g/cc
1.24 g/cc
catalyzed with QM CAT RED 3
1.24 g/cc
1.24 g/cc
catalyzed with QM CAT BLUE
1.28 g/cc
1.28 g/cc
Base
Viscosity 100 cP
100 cP
Uncatalyzed, QM CAT PURPLE
100 cP
100 cP
Uncatalyzed, QM CAT BLUE
100 cP
100 cP
Uncatalyzed, QM CAT RED 3
13500 cP
13500 cP
catalyzed with QM CAT RED 3
13500 cP
13500 cP
catalyzed with QM CAT BLUE
13500 cP
13500 cP
catalyzed with QM CAT PURPLE
20000 cP
20000 cP
Base
Linear Mold Shrinkage <= 0.0030 cm/cm

@Temperature 25.0 °C,
Time 259000 sec
<= 0.0030 in/in

@Temperature 77.0 °F,
Time 72.0 hour
Cured
Storage Temperature <= 38.0 °C
<= 100 °F
6 months
Mechanical Properties Metric English Comments
Hardness, Shore A 18
18
cured for 72 hrs @ RT
Tensile Strength, Yield 2.90 MPa
421 psi
cured for 72 hrs @ RT
Elongation at Break 500 %
500 %
cured for 72 hrs @ RT
Tear Strength 20.2 kN/m
115 pli
cured for 72 hrs @ RT
Processing Properties Metric English Comments
Dry Time 4 - 6 hour
4 - 6 hour
Demold time, catalyzed with QM CAT RED 3
12 - 16 hour
12 - 16 hour
Demold time, catalyzed with QM CAT PURPLE
16 - 24 hour
16 - 24 hour
Demold time, catalyzed with QM CAT BLUE
Cure Time 45.0 - 60.0 min
0.750 - 1.00 hour
Tack Free Time, catalyzed with QM CAT RED 3
240 - 360 min
4.00 - 6.00 hour
Tack Free Time, catalyzed with QM CAT PURPLE
360 - 480 min
6.00 - 8.00 hour
Tack Free Time, catalyzed with QM cat BLUE
Descriptive Properties Value Comments
Color Beige
Base
Blue
Uncatalyzed, QM CAT BLUE
Light Blue
catalyzed with QM CAT BLUE
Light Purple
catalyzed with QM CAT PURPLE
Light Red
catalyzed with QM CAT RED 3
Purple
Uncatalyzed, QM CAT PURPLE
Red
Uncatalyzed, QM CAT RED 3
Work Life 25 mins
catalyzed with QM CAT PURPLE
45 mins
catalyzed with QM CAT BLUE
7 mins
catalyzed with QM CAT RED 3
Users viewing this material also viewed the following: