3M Dyneon™ FC 2261Q Fluoroelastomer

Category Polymer , Thermoset , Fluoropolymer, TS , Rubber or Thermoset Elastomer (TSE)
Manufacturer 3M Dyneon™
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF 3M Dyneon™ FC 2261Q Fluoroelastomer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
3M™ Dyneon™ Fluoroelastomer FC 2261Q can be compounded using standard water cooled internal mixers or two-roll mills with standard fillers and ingredients utilized in typical fluoroelastomer formulations. The “dry” ingredients should be blended before adding to the masticated gum. For best results, Dyneon FC 2261Q should be banded on the mill several minutes prior to adding the blended dry ingredients. Once mixed, the compounded stocks have good scorch resistance and storage stability.Composition: di-polymer of vinylidene fluoride and hexafluoropropyleneProcess targets: compression moldingAmine or bisphenol curableIntermediate viscosity raw gumInformation provided by Dyneon, A 3M Company
Physical Properties Metric English Comments
Specific Gravity 1.80 g/cc
1.80 g/cc
Mooney Viscosity 63

@Temperature 121 °C
63

@Temperature 250 °F
ML1+10
Mechanical Properties Metric English Comments
Hardness, Shore A 77
77
Press Cure 5 minutes @ 177°C, Post Cure 24 hours @ 260°C; ASTM D2240
Tensile Strength at Break 12.9 MPa
1870 psi
Press Cure 5 minutes @ 177°C, Post Cure 24 hours @ 260°C
Elongation at Break 240 %
240 %
Press Cure 5 minutes @ 177°C, Post Cure 24 hours @ 260°C
100% Modulus 0.00434 GPa
0.630 ksi
Press Cure 5 minutes @ 177°C, Post Cure 24 hours @ 260°C
Compression Set 14 %
14 %
Aged 70 hours @ 200°C, -214 O-rings; ASTM D395 Method B
Thermal Properties Metric English Comments
Transformation Temperature -18.0 °C
-0.400 °F
TR10; ASTM D1329
Component Elements Properties Metric English Comments
Fluorine, F 65.9 %
65.9 %
Descriptive Properties Value Comments
Color Translucent to Off-White
MH, Maximum Torque 17 inch-lb
100 cpm, 0.5° Arc, 6 Minutes @ 177°C
ML, Minimum Torque 1.5 inch-lb
100 cpm, 0.5° Arc, 6 Minutes @ 177°C
Solubility Ketones and Esters
t`50, Time to 50% cure 2.5 minutes
100 cpm, 0.5° Arc, 6 Minutes @ 177°C
t`90 - Time to 90% cure 3.7 minutes
100 cpm, 0.5° Arc, 6 Minutes @ 177°C
ts2 - Time to 2 in-lb rise from min 1.9 minutes
100 cpm, 0.5° Arc, 6 Minutes @ 177°C