Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

3D Systems Accura® Bluestone™ Plastic for SLA® Systems

Category Polymer , Rapid Prototyping Polymer
Manufacturer 3D Systems Corporation
Trade Name Accura®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF 3D Systems Accura® Bluestone™ Plastic for SLA® Systems.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
A high stiffness engineered nanocomposite that opens new applications for stereolithography users. For use with solid-state stereolithography (SLA®) systems.ApplicationsWind-tunnel testing for the motorsports and aerospace industriesProduction of CMM/inspection and assembly jigs and fixturesLighting design and other applications where heat-generation from electrical components may be a factorCovers and enclosures of electrical and mechanical componentsWater-handling products, such as pump and impeller design or other componentsAutomotive "under-the-hood" applicationsHousings and enclosures that require high stiffness and rigidity, such as those for business machinesElectronic applications, such as insulating components, connectors, adaptor fittings, bases, sockets, and areas where ceramics might be usedAll information provided by 3D Systems.
Physical Properties Metric English Comments
Density 1.70 g/cc

@Temperature 25.0 °C
0.0614 lb/in³

@Temperature 77.0 °F
Liquid
1.78 g/cc

@Temperature 25.0 °C
0.0643 lb/in³

@Temperature 77.0 °F
Solid
Viscosity 1200 - 1800 cP

@Temperature 30.0 °C
1200 - 1800 cP

@Temperature 86.0 °F
Mechanical Properties Metric English Comments
Hardness, Shore D 92
92
Tensile Strength, Yield 66.0 - 68.0 MPa
9570 - 9860 psi
ASTM D638
Elongation at Break 1.4 - 2.4 %
1.4 - 2.4 %
ASTM D638
Tensile Modulus 7.60 - 11.7 GPa
1100 - 1700 ksi
ASTM D638
Flexural Strength 124 - 154 MPa
18000 - 22300 psi
ASTM D790
Flexural Modulus 8.30 - 9.80 GPa
1200 - 1420 ksi
ASTM D790
Izod Impact, Notched 0.130 - 0.170 J/cm
0.244 - 0.318 ft-lb/in
ASTM D256
Penetration 4.1
4.1
mils
Thermal Properties Metric English Comments
CTE, linear 33.0 - 44.0 µm/m-°C

@Temperature 0.000 - 20.0 °C
18.3 - 24.4 µin/in-°F

@Temperature 32.0 - 68.0 °F
T<Tg; ASTM E831-93
81.0 - 98.0 µm/m-°C

@Temperature 90.0 - 150 °C
45.0 - 54.4 µin/in-°F

@Temperature 194 - 302 °F
T>Tg; ASTM E831-93
Deflection Temperature at 0.46 MPa (66 psi) 65.0 - 66.0 °C
149 - 151 °F
ASTM D648
267 - 284 °C
513 - 543 °F
with 160ºC thermal postcure; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C
149 °F
ASTM D648
Glass Transition Temp, Tg 71.0 - 83.0 °C
160 - 181 °F
DMA, E"
Descriptive Properties Value Comments
Appearance Opaque blue
Critical Exposure (mJ/cm²) 6.9
Tested Build Styles EXACT™
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved